Hi Kevin!
That is exactly the part I'm talking about.
I finally was able to talk to an engineer at Littlefuse, and he said
that my cleaning process was too aggressive (I kind of expected that he
was going to say that). But he said that the little green plastic piece
has nothing to do with the function at all. He said it's just a cover
for the material beneath it, mainly to protect it during pick and place.
The plastic piece is attached to the part will a small dot of adhesive
which also has nothing to do with part function.
The "special Polymer composite" is the translucent milky looking stuff
on the sides. If you flipped the part upside down, you would see that
the whole bottom (except for the terminations) is made of this polymer.
The engineer told me that it basically operates like a bi-directional
zener diode and clamps the voltage. It doesn't light up, glow, or
anything...
I'm lowering the temps in the wash for these puppies and see if the
little green plastic doo-hickies stay on, or in your case Kevin, maybe I
got a bad batch...
Thanks for all the input everybody!
-Steve Gregory-
-----Original Message-----
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Monday, March 06, 2006 11:00 AM
To: [log in to unmask]; Stephen Gregory
Subject: RE: [TN] A new one for me, ESD Suppressors...
Steve,
Several years back we saw the same thing with the Littlefuse series PGB
ESD suppressors. We'd run them for a long time with no issues, then hit
a lotcode of parts where the green coating chipped or lifted off in the
process. Those assemlies were also seeing a fairly aggressive wash,
which included a saponified batch cleaning.
In the PGB series, I think that the round dots were a special composite
polymer and part of the ESD protection. The green coating was nothing
more than that. What we observed was that when the coating pulled away,
it sometimes removed or tore part of that polymer. We replaced any parts
with a non-intact coating.
Bruce Tostevin
Benchmark Electronics
Hudson, NH
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stephen Gregory
Sent: Monday, March 06, 2006 10:19 AM
To: [log in to unmask]
Subject: [TN] A new one for me, ESD Suppressors...
Mornin' Everybody!
Last Friday, I had a problem with a new part that I've never used
before, and maybe somebody else has seen this problem. It's with
something called an ESD Suppressor. It's a little 0603 SMT part that
looks a lot like a LED...in fact, that's what I thought it was at first.
It's made by Littlefuse.
My problem is that there's a little green piece of plastic on the top of
it that looks like it's held there with a tiny dot of glue, that is
either coming off or breaking during wash. I'm washing the boards in a
batch cleaner using Kyzen Aquanox 4512P at 140 F. for 20-minutes
followed by a ambient temperature rinse cycle, and a 15-minute 100 F.
dry cycle.
I did read in the datasheet that I'm probably washing at too high a
temperature. The datasheet says that they have been tested IAW ASTM-543
for 4-hours at 40 C., with 3 solutions (H2O, detergent solution, and a
defluxer). I didn't know that there was this limitation until we
observed the little green pieces of plastic coming off. You can see a
picture at:
http://stevezeva.homestead.com/files/ESD_Suppressor.jpg
My question is; what is that little green plastic piece? There's nothing
in the datasheet that describes it. Is it something functional to the
part? Or is it something there for pick and place? I've got a call into
Littlefuse and I'm just waiting for a call back. But I thought I'd ask
you all to see if someone else has run across these little guys before.
I don't have a clue about them...
Have a good Monday!
-Steve Gregory-
_______________________________________________________
This message may contain information that is privileged and confidential
to LaBarge, Inc. It is for use only by the individual or entity named
above. If you are not the intended recipient, you may not copy, use or
deliver this message to anyone. In such event, you should destroy the
message and kindly notify the sender by reply e-mail.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
_______________________________________________________
This message may contain information that is privileged and confidential to LaBarge, Inc. It is for use only by the individual or entity named above. If you are not the intended recipient, you may not copy, use or deliver this message to anyone. In such event, you should destroy the message and kindly notify the sender by reply e-mail.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|