I thought the SAC is more easy to oxidize...even after fluxing....I must be
wrong... thank Jason.
Best regards,
jk
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Jason Gregory
Sent: Thursday, October 13, 2005 5:52 PM
To: [log in to unmask]
Subject: Re: [TN] SAC reflow profile and flux vaporization
The manufacturer's recommended profiles are normally based on the flux used,
not really the alloy - the alloy has a lot to do with the profile, but the
flux has the most to do with style of reflow and they can be modified to
suit personal tastes and outcomes.
AIM actually suggests three scenarios ramp-to-spike, ramp-soak-spike, and
long soak - they are based on the WS flux we use.
Jason Gregory
Manufacturing Engineer
Innova Electronics
(281)653-5593
(281)653-5594 fax
(281)212-0844 cell
[log in to unmask]
-----Original Message-----
From: Joyce Koo [mailto:[log in to unmask]]
Sent: Thursday, October 13, 2005 4:34 PM
To: TechNet E-Mail Forum; Jason Gregory
Subject: RE: [TN] SAC reflow profile and flux vaporization
I thought SAC use ramp-to-spike...not ramp-soak-spike...may be just silly
me...jk
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Jason Gregory
Sent: Thursday, October 13, 2005 5:05 PM
To: [log in to unmask]
Subject: Re: [TN] SAC reflow profile and flux vaporization
Leo,
I use a different mfr. of SAC305 but I stay in the 60-90 sec for the
150-170c part of the profile. It works great for me. 160 seems very
excessive. Also, the 365 sec from ambient to reflow is long too. I stay with
4-4.5 min. (10 zone, 14 in. zone lengths at 32 ipm). If we find voiding at
the 5DX, I slow to 31 or 30.
Are they using ramp-to-spike or ramp-soak-spike?
Jason Gregory
Manufacturing Engineer
Innova Electronics
(281)653-5593
(281)653-5594 fax
(281)212-0844 cell
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leo Higgins
Sent: Thursday, October 13, 2005 3:51 PM
To: [log in to unmask]
Subject: [TN] SAC reflow profile and flux vaporization
Hello,
I have a case where a customer may be running an inappropriate reflow
profile for surface mounting on a board with and OSP pad finish. The
time/temp features of the profile push up against every min or max in the
recommended IPC reflow profile for SAC. The surface mount solder is
Sn-3Ag-0.5Cu (Senju 705). The time from 150-200C is 160 seconds (seems way
too long). The time from RT to peak is 365 sec. Time above 220C is 57
seconds. The solder shows wetting to the leadless contact on the package
and to the board, but temp cycle life is much less than normal. Solder
joint cross-sections show a atypically grainy structure and some show
microvoids dispersed across the joint. Looks to me like the flux was
vaporized before liquidus was reached, resulting in poor coalescence of
solder particles, further aggravated by a low peak temp of 234-235C. The
discussions about good SAC wetting on OSP needing 235-237C from Steve at
ClearCube add further concerns. The solder joints were somewhat
hour-glassed in cross-section so virtually all failures occurred through the
waist of the solder joint, so the impact of poor wetting was not seen, but
is not doubted. I think there are a number of possible problems with this
profile. Any comments? Specifically do you think the 160 sec. from
150-200C could have vaporized most of the flux?
Best regards,
Leo
Director of Applications Engineering
ASAT, Inc.
3755 Capital of Texas Highway, Suite 100
Austin, Texas 78704
ph 512-383-4593
fx 512-383-1590
[log in to unmask]
www.asat.com
The information contained in this electronic message is CUSTOMER/SUPPLIER
PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the
individual or entity named above. If the reader of this message is not the
intended recipient, you are hereby notified that any dissemination,
distribution and copying of this communication is strictly prohibited. If
you have received this communication in error, please immediately notify the
sender by electronic mail. Thank you.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per
day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|