TECHNET Archives

October 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
Leo Higgins <[log in to unmask]>
Date:
Wed, 19 Oct 2005 16:30:17 -0700
MIME-Version:
1.0
X-To:
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Leo Higgins <[log in to unmask]>
Parts/Attachments:
text/plain (85 lines)
Hi Werner,
     So since the CTEs of the matls involved are different, as are the
materials used in other elements of the substrate of similar dimensions,
would it be correct to say...(1) the adhesion of the Cu to the fill should
be high enough to elastically tolerate the CTE mismatch without delam; or,
(2) this separation due to 'resin recession' is typical and is not a
reliability risk?  We and the customer are tending to go with (1).


Best regards,
Leo

Director of Applications Engineering
ASAT, Inc.
3755 Capital of Texas Highway, Suite 100
Austin, Texas     78704

ph     512-383-4593
fx      512-383-1590
[log in to unmask]
www.asat.com


The information contained in this electronic message is CUSTOMER/SUPPLIER
PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the
individual or entity named above. If the reader of this message is not the
intended recipient, you are hereby notified that any dissemination,
distribution and copying of this communication is strictly prohibited. If
you have received this communication in error, please immediately notify the
sender by electronic mail. Thank you.



-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Werner Engelmaier
Sent: Wednesday, October 19, 2005 6:15 PM
To: [log in to unmask]
Subject: Re: [TN] Delamination at Thermal Via area?


In a message dated 10/19/05 17:23:15, [log in to unmask] writes:
> Hi Leo!
>
> Your pics are up! Go to:
>
> http://www.stevezeva.homestead.com/files/Delam_in_Via.jpg
> http://www.stevezeva.homestead.com/files/Dalam_in_Via_Close.jpg
>
 Hi,
What this pics show is a classical case of 'resin recession.' It happens
with
PTV-barrels all the time; however, the term 'resin recession' is a misnomer.
During excursion to soldering T's, the polymeric fill will expand more than
the Cu-barrel and push the Cu-caps outward plastically deforming them. On
cooling, the resin 'recedes' to its original volume, the plastically
deformed Cu
cannot follow, and you have this classic case of 'resin recession.'


Werner

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2