Steve,
I agree with the comments below. The boards should be rejected due to air
entrapment. Essentially you have solder mask that has no adhesion to the
base material and will most likely fail during thermal stress. Dry film
solder mask is brittle in nature and without complete adhesion to the base
laminate, this is a failure waiting to happen.
Bob Metcalf
Circuit Solutions
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Brummer Chuck
Sent: Thursday, June 02, 2005 10:49 AM
To: [log in to unmask]
Subject: Re: [TN] Dry Film Soda Strawing...
Steve,
I think that if you call this soda straw you are being to kind. Depending
on the inspector this is "Air Entrapment" or "Delamination". I think it
will get worse with further heat cycling and the mask might even break and
chip away.
Reject it is my thought.
Chuck Brummer
Siemens Medical Solutions
-----Original Message-----
From: Stephen Gregory [mailto:[log in to unmask]]
Sent: Thursday, June 02, 2005 7:51 AM
To: [log in to unmask]
Subject: [TN] Dry Film Soda Strawing...
Mornin' all ya'll...
We've got some boards in here with dry-film mask "soda strawing".
I've got pictures up on my page at: http:// www.stevezeva.homestead.com
and look at "Soda Strawing, Soda Strawing 2, 3, and 4".
These are class 3 boards and I say that if there's any evidence of soda
strawing
it's nonconforming, no matter if the soda straw is completely sealed or
even if it
doesn't reduce the conductor spacing below the minimum requirements.
If you see it on a class 3 board, it's rejectable according to the IPC-600G
is the way I
read it...am I wrong?
BTW, I'm definately rejecting the board in the picture "Soda Strawing 4".
That picture
is over a planar transformer pattern and has the trace exposed. The other
three pictures
are the different degrees of soda strawing that I'm seeing...is any of it
acceptable?
Kind regards,
-Steve Gregory-
Senior Process Engineer
LaBarge Incorporated
Tulsa, Oklahoma
(918) 459-2285
(918) 459-2350 FAX
__________________________________________________________________
This message may contain information that is privileged and confidential to
LaBarge, Inc. It is for use only by the individual or entity named above.
If you are not the intended recipient, you may not copy, use or deliver
this message to anyone. In such event, you should destroy the message and
kindly notify the sender by reply e-mail.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|