TECHNET Archives

April 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-type:
text/plain; charset=us-ascii
Sender:
Subject:
From:
Stephen Gregory <[log in to unmask]>
Date:
Thu, 21 Apr 2005 10:35:45 -0500
MIME-Version:
1.0
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Ingemar Hernefjord (KC/EMW)" <[log in to unmask]>
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Parts/Attachments:
text/plain (103 lines)
Hi Inge!

Your pictures are up! Go to:  http://www.stevezeva.homestead.com  and look
for; "PWB Fresh, and PWB Used".

That is pretty weird looking! Is that the white stuff you were talking
about  where
you printed your last name?

I've never used any teflon fabs here, so I don't have a clue about them...

Kind regards,

-Steve Gregory-
Senior Process Engineer
LaBarge Incorporated
Tulsa, Oklahoma
(918) 459-2285
(918) 459-2350 FAX


|---------+--------------------------------->
|         |           "Ingemar Hernefjord   |
|         |           (KC/EMW)"             |
|         |           <ingemar.hernefjord@ER|
|         |           ICSSON.COM>           |
|         |           Sent by: TechNet      |
|         |           <[log in to unmask]>     |
|         |                                 |
|         |                                 |
|         |           04/21/2005 09:49 AM   |
|         |           Please respond to     |
|         |           TechNet E-Mail Forum; |
|         |           Please respond to     |
|         |           "Ingemar Hernefjord   |
|         |           (KC/EMW)"             |
|         |                                 |
|---------+--------------------------------->
  >--------------------------------------------------------------------------------------------------------------|
  |                                                                                                              |
  |       To:       [log in to unmask]                                                                              |
  |       cc:                                                                                                    |
  |       Subject:  [TN] Copper traces too, but Rogers this time                                                 |
  >--------------------------------------------------------------------------------------------------------------|




Hi all,
anyone who have this experience?
A. Peel fresh PWB: high force needed, white stuff left on board. Soft like
butter. Copper underside yellowish.
B. Peel used PWB: much lower force needed, no white stuff left on board.
Copper underside brown-blue-redish.

Reason for asking is this. We suspect that something bleeds out from
beneath the copper traces during the
VIGON cleaning. Not much, but sometimes creating kind of 'grease' along the
copper traces. Therefore, I'm
interested in the interface between the copper and the teflon. What stuff
can there be that changes from white to colourless, and may be dissolved by
VIGON.

Sending two pics to the always and amazingly tolerant, patient and positive
S.G.

Ingemar Hernefjord
Ericsson Microwave Systems

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------




__________________________________________________________________
This message may contain information that is privileged and confidential to
LaBarge, Inc.  It is for use only by the individual or entity named above.
If you are not the intended recipient, you may not copy, use or deliver
this message to anyone.  In such event, you should destroy the message and
kindly notify the sender by reply e-mail.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2