TECHNET Archives

November 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="ISO-8859-1"
Sender:
Subject:
From:
"Ingemar Hernefjord (KC/EMW)" <[log in to unmask]>
Date:
Thu, 25 Nov 2004 09:12:59 +0100
MIME-Version:
1.0
X-To:
TechNet E-Mail Forum <[log in to unmask]>, - Bogert <[log in to unmask]>
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Ingemar Hernefjord (KC/EMW)" <[log in to unmask]>
Parts/Attachments:
text/plain (64 lines)
Whiskers! Horror! I've been in this mess recently. Lots of expensive waveguides had to be reworked, cause the insertion loss became a catastroph at this wavelength. NASA have some of my pics:
http://nepp.nasa.gov/whisker/photos/waveguide/index.html
This was a product of unawareness about tin plating nature from both sides, both us as buyer and waveguide manufacturer. This happens to the best when in hurry. Now, to your specific headache. The whiskers can grew several millimeters in just some weeks! When we applied the power pulses some whiskers burnt off, but new came instead. There were hundreds and hundreds new whisker babies ready to grew and become 10 mm long and proud whisker adults. I took one waveguide flange, dipped it in liquid nitrogen, heated it with a hairblower, repeated this a couple of times and could see how they grew. To get rid of them, we could eliminate the built-in tension by simply reflowing the tin layer, but it was impractical as the waveguides had silicon rubber on the outside. Instead we dipped the waveguide flanges (the whiskers appeared only in and on the flanges)for some seconds in an acid mixture and clean carefully. The babies vanished, the superficial tin layers were relaxed, and the par!
 ts could be used again. Experimentally succesful, but we didn't use these parts for series production.
Home lesson?....Tin on flanges was banned, of course.

Additional: the guys at NASA are whisker gurus, call Jay Brusse, for instance.

Ingemar Hernefjord
Ericsson Microwave Systems



-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of - Bogert
Sent: den 24 november 2004 21:43
To: [log in to unmask]
Subject: [TN] Tin whiskers


November 24, 2004

We have experienced problem with power planes (laminated bus assemblies) that have embedded copper planes it them with electrical boss connections brazed thereto.  The copper planes are laminated together in an operation similar to a PWB.  Epoxy is then added to the assembly via the edges.  The process produced voids.  These voids, in conjunction with the tin whiskers that grew from the tin-plated copper, caused short-circuit.  Although the tin whiskers vaporized from the short-circuit energy available from large capacitors, an arc was sustained that ultimately cleared some fuses.

Our equipment initially passed 3500 VDC dielectric strength test and functional test of the equipment.  However, after about a year in storage (no voltage applied), the equipment failed when 700 VDC was initially applied.  We also did dielectric test on some power planes that were not assembled yet.  The product failed the first time.  However, when the dielectric test was repeated, it did not fail second time.

Bottom line is that we believe tin whiskers grew in the internal epoxy voids and ultimately caused short circuit.

Our solution to justify continued use of previously built product was to retest at 1,000 VDC for all product that was not energized for at least a six month period.  We also redesigned the power plane for new product.

My question is, what happens to tin whiskers once they are vaporized by short-circuit current?  What is the residue that results (some form of tin)?  I assume it is still conductive.  If we do the dielectric test at 1000 VDC, will it destroy all tin whiskers after six months, or will more grow?

Will the vaporized tin whiskers form a conductive film within the epoxy void such that we could still get a short-circuit?

I recognize that one does not need voltage to cause tin whiskers.  However, if tin whickers exist with no voltage applied, will they grow larger if we apply a voltage (700 VDC)?

I have read papers regarding how to preclude tin whiskers.  Some papers indicate that a coating of conformal coating or epoxy that is 0.006 inch thick will prevent whiskers.  Other papers indicate that this only slows whisker growth but does not prevent it.

Some papers indicate that nickel plate under the tin, or annealing after plating at 200C will stop whiskers.

Some papers indicate that doping the tin with 3 % lead will prevent whiskers.  However, other papers indicate one can get whiskers at higher lead doping rates.

What is the best way to prevent whiskers from forming in tin plated
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
copper bus bars?

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2