Everyone is saying inadequate glass etch but few fabricators these days are
really using a glass etch. Drilling doesn't look good, but I'd say it's
over-aggressive desmear. That's why so much glass fiber protrusion.
Franklin, what was desmear condition? Alkaline permanganate? How long, what
temp.? One-pass or two? Is it ordinary FR-4, high Tg, or more high
performance material?
The plating definitely looks thin, based on comparison with inner foil,
whether it's 1 oz. or 1/2 oz.
Tim Reeves
Tyco Printed Circuit Group - Dallas Division
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Werner Engelmaier
Sent: Tuesday, March 30, 2004 9:08 AM
Subject: Re: Hole wall quality
Hi Franklin,
Whether or not these PWBs will give trouble in service depends on the
product
appllication--o.k. for benign environments, likely to fail in servere
environments. The certainly are not the prettiest x-sections I have
seen--inadequate
glass etch, some glass-fiber rip-out, l plating rather thin---all resulting
in
stress risers in thin plating that is thinner still localized.
Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|