Technet,
I have come across a rash of failed assemblies that have 0805 capacitors
and resistors, bottom side glued, wave soldered and washed. Trouble
shooter reported touching up the solder joints on a few areas and the
boards would pass test.
I had a look at one board which was reported to have a 0805 56K resistor
with "drifting" values. I pulled the component off mechanically in order
not to apply any heat and noticed several mini-voids within the adhesive
body. I have seen solder bridge within the glue before but this was the
first time I saw wet residue within the voids.
You can view a sample image from Steve's web site:
http://www.stevezeva.homestead.com/files/SMTAdhesive.jpg
The image showed the bottom side of the cracked resistor after removal
(white), with a portion of solder mask (green) and SMT adhesive (red).
I used a 8mil stencil. The thermal profile was verified and conformed to
the slope/ curing specs.
Has anyone seen this before? Any explanation as to how the void was
formed and how moisture got tapped in? Does anyone re-use their glue on
the line or throw away any left-over to avoid moisture in the glue?
Rgds,
Peter
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|