Hi Dan! I cheated - I had two donuts! I should have given a better
explanation. The solderability issues I have experienced originate from an
improper tinning of the filter leads which were the 770 alloy. The improper
coating resulted in oxidation of the 770 surface which our low residue flux
materials could not adequately remove to permit the creation of a reliable
solder joint. Using an OA flux we were able to get a properly tinned
surface on the filters which then soldered without issue in production. I
haven't seen any issues with the 770 alloy (either first or second pass)
provided the initial solder coating was done correctly. Question for you -
it seems like many filter fabricators use 7XX alloys - is there an
electrical advantage to use those alloys or is it a material formability
advantage?
Dave
"Dan R. Johnson"
<[log in to unmask] To: [log in to unmask]
> cc:
Sent by: TechNet Subject: Re: [TN] German Silver
<[log in to unmask]>
03/12/2003 10:07
AM
Please respond to
"TechNet E-Mail
Forum."; Please
respond to "Dan
R. Johnson"
Hi Dave,
Hope you enjoyed the doughnut, I'm sipping bad coffee with sweet and low :
(
A question about the filters you mentioned. We use alloy 770 and 752 for
our
Rf Shields, I have never seen a solderability issue.
Even stock that was over five years old soldered great. What causes poor
solderability with the filters? Is it a "second pass" phenomena?
Dan
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|