Stu,
I have not found a need to add solder paste for BGA replacements of any size
and use flux only, typically No Clean. I do prefer to leave an extremely
small dome of solder on each pad as part of pad prep to ensure no exposed
intermetallic and enhance wetting. We accomplish this under a microscope
and perform a 10X visual prior to placement of the new part with a Sniper
System (TM). We have had excellent success with the exception of the Altera
part with the known warpage problem.
Regards,
Bruce Misner
> ----------
> From: [log in to unmask][SMTP:[log in to unmask]]
> Reply To: TechNet E-Mail Forum.;[log in to unmask]
> Sent: Tuesday, May 14, 2002 10:34 AM
> To: [log in to unmask]
> Subject: [TN] BGA replacement
>
> The M.E.s at my company are struggling with replacing a defective plastic
> BGA.
> We have an Air Vac BGA machine. The lead M.E. feels that he needs a solder
> pad
> deposit in place before putting the replacement BGA on the board for
> reflow. He
> feels that he will compensate for irregular solder balls on the part and
> also
> possible surface differences on the existing pads which have been wicked
> clean
> of solder.
>
> The problem is in putting down the paste. He is teaching a technician to
> use a
> small medium stiff plastic stencil. The paste is applied with a wide
> chisel
> blade x-acto knife looking tool. They are getting uneven solder cakes and
> icicles between the solder deposits.
>
> I ask, is that the best way to put down paste? Is it necessary on a
> plastic BGA
> to put down a paste deposit? Will the stringers pull in when heated or
> will they
> results in shorts after reflow?
>
> Any info appreciated.
>
> Thanks,
>
> Stu Korringa
> Quality Engineer
> Smiths Industries Electronic Systems
> Grand Rapids, Mi.
>
>
> **********************************************************************
> This e-mail and any files transmitted with it are confidential and may
> be legally privileged or otherwise exempt from disclosure under
> applicable law. This e-mail and its files are intended solely for
> the individual or entity to whom they are addressed and their content
> is the property of Smiths Aerospace. If you are not the intended
> recipient, please do not read, copy, use or disclose this communication.
> If you have received this e-mail in error please notify the e-mail
> administrator at [log in to unmask] and then delete this e-mail, its
> files and any copies.
>
> This footnote also confirms that this e-mail message has been scanned
> for the presence of known computer viruses.
> ***********************************************************************
>
> --------------------------------------------------------------------------
> -------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
> SET Technet NOMAIL
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> --------------------------------------------------------------------------
> -------
>
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|