hi,
assumption #1.- this is a through hole solder joint.
assumption #2.- this ring is on the 'top' side
assumption #3.- the connector leads are solderable
assumption #4.- the flux wetted the top-side pad and the lead.
assumption #5.- you are using a wave solder machine to make this solder joint
sounds like you haven't gotten enough preheat and/or the belt speed is too slow. if the assumptions aren't correct, disregard this email.
phil
-----Original Message-----
From: Jean-Francois Bissonnette [mailto:[log in to unmask]]
Sent: Thursday, April 20, 2000 3:29 PM
To: [log in to unmask]
Subject: [TN] Solder fillet problem
Hi All!
Probably too late to ask but I need some input for this
weard problem.
I got some connector with big leads that, with the unaided
eye looks properly soldered. But if I look at it with the
microscope at 10X, it looks like the fillet does not realy
stick to the lead. The fillet end rather abrubtly (makes a
rign) and it looks like there was no fusion between the lead
and the solder. I hope my explanation is clear enough!!!
JF
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|