TECHNET Archives

March 2000

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Brian Ellis <[log in to unmask]>
Date:
Thu, 2 Mar 2000 20:26:45 -0000
Reply-To:
Michael Fenner <[log in to unmask]>
Subject:
From:
Michael Fenner <[log in to unmask]>
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="iso-8859-1"
Organization:
Bonding Services & Products
MIME-Version:
1.0
Parts/Attachments:
text/plain (155 lines)
I think perhaps this response may be a little harsh...
A water break test is a reasonable test not for the cleanliness of a surface but its ability to
be wetted by water.
True it is wrong to extrapolate from this to assume that if water can wet the surface then
everything else will, also it should be kept in context.
Personally I think it is not too bad a guide for paints, some adhesives and so on when used on
metal surfaces, especially if it is used before and after cleaning. I agree it is pretty useless
for other purposes such as solderability plating and so on.

Mike

----- Original Message -----
From: Brian Ellis <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, March 01, 2000 4:08 PM
Subject: Re: [TN] How to detect contamination on metal surface


> Rainer
>
> I'm sorry, but the so-called water-break test is as useless as the name is long. It is
> one of the biggest myths and fallacies that occurs in our industry and should be
> drowned in the water required for it and then laid to permanent rest.
>
> Proofs:
> 1) Take some new blown glass, as soon as it cools: it dewets in pure water: therefore
> it is contaminated, according to your theory. Wash and rinse it in a household
> dishwashing fluid: it wets: therefore it is clean according to your theory. The
> difference: some surfactant is contaminating the surface in the second case.
>
> 2) Take a freshly vacuum deposited copper mirror: it dewets in pure water:  therefore
> it is contaminated, according to your theory. Leave it lying around for a few days to
> nicely oxidise: it wets: therefore it is clean according to your theory. The
> difference: the oxidateion is more hydrophilic than the bare metal.
>
> 3) Vacuum deposit copper on a smooth glass slide and on a piece of heavily frosted
> glass (not too thick a deposit though). The smooth glass mirror dewets: therefore it is
> contaminated, according to your theory. The rough copper wets:  therefore it is clean
> according to your theory. In fact, they have identical levels of cleanliness. The
> difference: the surface tension of the water holds it in place much better on the rough
> surface.
>
> All these comparisons should be done with the purest water because tap water will
> contain an unknown soup of things which will alter the surface tension and therefore
> might change the results significantly. In fact, if you study the action of soaps and
> detergents, as well as any micellar or non-micellar tensio-active surface agent (which
> are found in most water including DI), you will understand that a wetting surface
> probably means that the surface has, at some time in its history, been subjected to
> such a substance.
>
> Refs: Surface Phenomena by S.R. Rao, Hutchinson Educational Ltd, ISBN 0 09 112300 3
> Any work by K.L. Mittal including his collected Treatise on Clean Surface Technology
> Volumes 1 and 2, Plenum Publishing, ISBN 0-306-42420-7
> And dare I mention it without getting flamed for publicity?, my own book specifically
> for the electronics industry.
>
> Can we please lay this old red herring to its well deserved and everlasting rest?
>
> Brian
>
>
> "Blomberg, Rainer (FL51)" wrote:
>
> > Marvin,
> >
> > A simple test for cleanliness is what we call the "water break free" test.
> > Apply D.I. water to the surface to be tested and observe how well the water
> > wets the surface.  It should flow out, onto the surface and not bead up
> > (like on a waxed surface).  As the water flows off the surface, when the
> > sample is held vertical, it should sheet off in a thin film and not bead on
> > the surface for 5-10 seconds.  Another method is to apply a few drops to the
> > horizontally held surface and judge the angle the meniscus makes.  The
> > cleaner the surface, the shallower the angle.  As for identifying the
> > contamination, we typically use SEM and IR Spectroscopy.
> > Hope this helps.
> >
> > -----Rainer Blomberg
> >
> > -----Original Message-----
> > From: marvin v. picardal [mailto:[log in to unmask]]
> > Sent: Wednesday, March 01, 2000 6:34 AM
> > To: [log in to unmask]
> > Subject: [TN] How to detect contamination on metal surface
> >
> > Dear Techneters,
> >
> > I would like to ask some information as to
> > how to detect contamination on metal surface and
> > how do I determine what type of contamination that is.
> > The said contamination results to poor adhesion
> > between the glue and the metal surface.
> >
> > I do hope you would take time in helping me out with this.
> > Thank you in advance.
> >
> > Marvin
> >
> > ##############################################################
> > TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> > ##############################################################
> > To subscribe/unsubscribe, send a message to [log in to unmask] with following
> > text in
> > the body:
> > To subscribe:   SUBSCRIBE TECHNET <your full name>
> > To unsubscribe:   SIGNOFF TECHNET
> > ##############################################################
> > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> > information.
> > If you need assistance - contact Keach Sasamori at [log in to unmask] or
> > 847-509-9700 ext.5315
> > ##############################################################
> >
> > ##############################################################
> > TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> > ##############################################################
> > To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
> > the body:
> > To subscribe:   SUBSCRIBE TECHNET <your full name>
> > To unsubscribe:   SIGNOFF TECHNET
> > ##############################################################
> > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> > information.
> > If you need assistance - contact Keach Sasamori at [log in to unmask] or
> > 847-509-9700 ext.5315
> > ##############################################################
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
> the body:
> To subscribe:   SUBSCRIBE TECHNET <your full name>
> To unsubscribe:   SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> information.
> If you need assistance - contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> ##############################################################
>

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################

ATOM RSS1 RSS2