从照片上看象是白斑。微裂纹和白斑的外观区别主要是分散状态还是连成一片。原因可能是你在压入插针时,在层压板内层产生的应力,受热后发生了内部分层。如果想更准确地确认和进行原因分析,建议做剖面分析。
Best Regards,
NEW:10月25-29日深圳 IPCWorks Asia众多技术活动期待您参与!
James Liu 刘春光
Director, Industry Programs 工业项目总监
IPC China
[cid:[log in to unmask]]
北京市经济技术开发区宏达北路18号大地国际大厦407A
Suite 407A,Dadi international Building, #18 Hongda North Rd., BDA 100176 Beijing China
Tel: +86 10 67885326
Fax: +86 10 67885326
MP: +86 136 0133 3491
[log in to unmask]<mailto:[log in to unmask]>
www.ipc.org.cn<http://www.ipc.org.cn>
发件人: TGAsia [mailto:[log in to unmask]] 代表 Wang, Jennifer
发送时间: 2010年9月30日 10:19
收件人: Listserv TGAsia
主题: Re: [TGAsia] 请教:此种情况是IPC-A-610D中的白斑还是微 裂纹
各位坛友
今日在生产过程中,看到了一个现象,就此异常现象是属于白斑还是微裂纹产生了争议,照片如下。
附件中可见的焊点为压接的插针;整个PCBA有压接插针的地方有如图所示的异常情况,其它焊接点周围及板面正常。
在试验过程中,插针压接在PCB上以后,并无白斑或微裂纹等异常情况;当过完波峰焊之后,如图所示的情况就出现了。请问此种情况是应属于白斑还是微裂纹?
此种异常情况出现的可能原因有哪些?(注:插针压接及波峰焊过程我们试验过程都做了记录,没有异常)
请指教!
[cid:[log in to unmask]]
王萍
________________________________
*** Confidentiality Notice: This e-mail, including any associated or attached files, is intended solely for the individual or entity to which it is addressed. This e-mail is confidential and may well also be legally privileged. If you have received it in error, you are on notice of its status. Please notify the sender immediately by reply e-mail and then delete this message from your system. Please do not copy it or use it for any purposes, or disclose its contents to any other person. This email comes from a division of the Invensys Group, owned by Invensys plc, which is a company registered in England and Wales with its registered office at 3rd Floor, 40 Grosvenor Place, London, SW1X 7AW (Registered number 166023). For a list of European legal entities within the Invensys Group, please click this Link<http://www.invensys.com/legal/default.asp?top_nav_id=77&nav_id=80&prev_id=77.>.
You may contact Invensys plc on +44 (0)20 3155 1200 or e-mail [log in to unmask]<mailto:[log in to unmask]>. This e-mail and any attachments thereto may be subject to the terms of any agreements between Invensys (and/or its subsidiaries and affiliates) and the recipient (and/or its subsidiaries and affiliates).
________________________________
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|