TECHNET Archives

May 2007

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Thu, 31 May 2007 10:35:31 +0300
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Reuven Rokah <[log in to unmask]>
Subject:
From:
Reuven Rokah <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (73 lines)
Hi Werner,
If class 1 is accepting 50% filling of through holes with solder and
class 3 is accepting full PTH, I hope you agree that the solder joints
strength are not the same?

What I wanted to clarify, is that with lead free process, beside the
known failures such whiskers, lifted pads etc., the DOA / short terms
failures are mostly bad solder joints (SMT and through holes) happened
because the small process window (PCB and components finish type / i.e
short storage / shelf life and hi peak temperature). 

I have seen lot of reliability tests evaluation of Lead free including
life cycles, talking about the difference between the alloys.  I didn't
see lot of tests evaluation dealing about the bad solder joints / low
yield happened because the small process window.

Best Regards
Reuven ROKAH 
e mail: [log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Thursday, May 31, 2007 12:30 AM
To: [log in to unmask]
Subject: Re: [TN] RoHS compliant laptop with early failure

Hi Reuven,
Actually, it is not quality but inadequate or non-existant DfR [design
for 
Reliability]. Solder joints are subject to the same creep-fatigue
whether they 
are Class 1 or Class 3-the difference may be that the operational
environment 
may-may- be more severe for Class 3 product. But I have seen Class 1, or
more 
accurately Class 0 (Class minus 1?) [unsupported holes] in automotive 
under-the-hood environments.

Werner



**************************************
 See what's free at http://www.aol.com.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2