Rod:
The guidelines we have established here are as follows:
Total combined voiding <25%
Less than or equal to 3 separate voids
No two voids can intersect, irrespective of size/percentage
Another 2cents...
> -----Original Message-----
> From: Rod Martens [SMTP:[log in to unmask]]
> Sent: Wednesday, October 07, 1998 2:48 PM
> To: [log in to unmask]
> Subject: Re: [TN] Voiding in BGA
>
> I've never seen an exact number for voiding, but would be interested
> if anyone
> does have one. As for personal experience, we have seen cases where a
> single
> large void or many small voids aligned at an interface negatively
> impacted the
> reliablility. Also, we saw a case where some degree of voiding
> actually
> increased the life of BGA's, most likely due to some sort of crack
> arrest
> mechanism. I would imagine that a good number for max. voiding would
> need to
> include not just % void, but also position in the joint.
> My $0.02,
> Rod Martens
>
> -----Original Message-----
> From: Non-HP-FEiranova
> /hp-ftcollins,[log in to unmask]
> Sent: Wednesday, October 07, 1998 2:39 PM
> To: Non-HP-TechNet /hp-ftcollins,[log in to unmask]
> Cc: Non-HP-FEiranova
> /hp-ftcollins,[log in to unmask]
> Subject: [TN] Voiding in BGA
>
> To all:
> Is there a specification to address the maximum voiding allowed
> for PBGA and CBGA solder joints attached to FR-4 substrate ?
> Can anybody share some personal experiences in this matter ?
> Thanks
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV
> 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following
> text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
> section for
> additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or
> 847-509-9700
> ext.312
> ################################################################
> << File: [TN] Voiding in BGA.TXT >>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|