Hi Peter,
What I am saying is, that "barrel cracking is now the more common problem in
small-diameter holes, that the "non-functional pad" issue has fallen off in
importance and that n-f pads do not contribute to barrel cracking."
Small-diameter holes are more prone to barrel cracking, which is caused by
the z-axis expansion of the resin. Thin, non-uniform and low-ductility Cu
plating, as well as high resin content and low Tg, and of course PCB
thickness and Tmax all contribute to the possibility of barrel cracking. The
presence of n-f lands replaces some of the resin, which has some but not a
significant positive effect.
Larger diameter holes are more prone to inner-layer [post] separation. Thin
Cu plating, as well as high resin content and low Tg, and of course PCB
thickness and Tmax all contribute to the possibility of ILS; further bad or
thin Cu foil as well as low quality wet processing also are an issue. The
absence of n-f lands increases resin recession, but not necessarily ILS.
>How then to support hole plating and prevent its deformation through resin
recession and/or >hole pull-away?
****You got it backwards--barrel hole wall is deformed during resin
expansion; when the resin cools and returns to its initial volume, the
plastically deformed Cu cannot follow and 'resin recession' or 'hole
pull-away' results.
>Or are these defects not significant in purely interconnect via holes?
**** 'Resin recession' or 'hole pull-away' are not real reliability issues
either for vias or PTHs.
>Is removal of n-f pads to prevent barrels cracking better than keeping them
to give support
>to the barrel plating?
****As I said, n-f pads do not significantly affect barrel cracking one way
or the other. If processing problems are not an issue, I would keep the n-f
pads, however.
>Do you know what, if any, correlation there is between plating thickness,
>hole diameter, aspect ratio, number of layers and the point where barrel
>cracking becomes more prevalent and hole pull-away/resin recession becomes
>less significant?
****Aspect ratio is a 'red flag' indicator, not a real parameter. However,
for barrel cracking the correlation between plating thickness, hole diameter,
PCB thickness, resin Tg and T-excursion exists and has been modeled. For ILS
the correlation is qualitative, but not quanitative.
I had hoped to deal with some of these issues in workshops in Singapore,
which because of the SARS issue I had to postpone.

Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL  32174  USA
Phone: 904-437-8747, Fax: 904-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2