Hi Phil: I believe you will find either Phosphorous or Boron present in
all electroless nickel. Depending on the type of EN plating bath, either
sodium hypophosphite, sodium borohydride or dimethylamine borane are
used as reducing agents.
EN and electroplated nickel as a final finish are both solderable if you
use a hot enough flux. However there is nothing special about the
presence of P or B in the EN plating that will make it a magically
solderable final finish for electronic applications where super active
fluxes are not acceptable.
However the P and B concentrations will change the physical properties.
And yes the proper P content is important when specifying EN under IG
for electronics.
Regards
Michael Barmuta
Fluke Corp.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Crepeau, Phil (Space
Technology)
Sent: Tuesday, March 28, 2006 7:40 AM
To: [log in to unmask]
Subject: Re: [TN] Nickel Lead Finish
hi,
this is pretty fuzzy to me, but it seems to me that there was (early
1970's) an electroless nickel/phosphorus and electroless nickel/boron
finish that was touted as being solderable. could this be enjoying a
lead-free renaissance?
phil
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Barmuta, Mike
Sent: Tuesday, March 28, 2006 7:15 AM
To: [log in to unmask]
Subject: Re: [TN] Nickel Lead Finish
Hi Ken: Yes you should be concerned. As others have said Ni can be very
difficult to solder to. We've been down this Ni final finish road
before. In one case we had to tin the leads to get acceptable results,
in another we changed suppliers to get the finish we wanted.
What type of flux are you using in your solderpaste for the SM assembly
process? If it's no-clean you will probably have trouble. If it's WS
then you "might have a chance. However in either case it will require
longer dwell times above liquidious.
Are you sure the supplier will not be putting a solderable finish over
the nickel? If possible I would specify a matte tin over Ni finish. This
would provide much better solderability, still be RoHS compliant for the
component manufacturer and the lead in your solder would prevent whisker
formation.
The only issue may be acceptance of a pure tin finish from your
customers in aerospace. If they won't accept it then change to a
component supplier that can give you the finish you want.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bloomquist, Ken
Sent: Tuesday, March 28, 2006 6:11 AM
To: [log in to unmask]
Subject: [TN] Nickel Lead Finish
We were just notified by one of our capacitor manufacturers that they
were going lead free and their replacement finish will be nickel. These
are surface mount parts.
If my memory serves we had trouble soldering nickel leads some years ago
on some TO-5 parts.
We are a class 3 manufacturer and will continue to use lead in our
solder. Should we be concerned about the solderability of the nickel
lead finishes?
Thanks,
KennyB
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
This message (including any attachments) contains confidential and/or
proprietary information intended only for the addressee.
Any unauthorized disclosure, copying, distribution or reliance on the
contents of this information is strictly prohibited and may constitute a
violation of law. If you are not the intended recipient, please notify
the sender immediately by responding to this e-mail, and delete the
message from your system. If you have any questions about this e-mail
please notify the sender immediately.
Ce message (ainsi que les eventuelles pieces jointes) est exclusivement
adresse au destinataire et contient des informations confidentielles. La
copie, la communication ou la distribution du contenu de ce message sans
l'accord prealable de l'expediteur sont strictement interdits et peuvent
constituer un delit. Si vous n'etes pas destinataire de ce message,
merci de le detruire et d'avertir l'expediteur. Si vous avez des
questions se rapportant a ce courrier electronique, merci de bien
vouloir notifier l'expediteur immediatement.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
This message (including any attachments) contains confidential
and/or proprietary information intended only for the addressee.
Any unauthorized disclosure, copying, distribution or reliance on
the contents of this information is strictly prohibited and may
constitute a violation of law. If you are not the intended
recipient, please notify the sender immediately by responding to
this e-mail, and delete the message from your system. If you
have any questions about this e-mail please notify the sender
immediately.
Ce message (ainsi que les eventuelles pieces jointes) est
exclusivement adresse au destinataire et contient des
informations confidentielles. La copie, la communication ou la
distribution du contenu de ce message sans l'accord prealable de
l'expediteur sont strictement interdits et peuvent constituer un
delit. Si vous n'etes pas destinataire de ce message, merci de le
detruire et d'avertir l'expediteur. Si vous avez des questions se
rapportant a ce courrier electronique, merci de bien vouloir
notifier
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
l'expediteur immediatement.
|