David Hillman <[log in to unmask]>
Reply To:
TechNet E-Mail Forum.
Date:
Fri, 16 Nov 2001 12:17:40 -0600
Content-Type:
text/plain
Parts/Attachments:
text/plain (286 lines)
Hi folks! Intermetallic layers are alloys (at least per the ASMI definition
of an "alloy") but that is another discussion topic. Eric - take a look
section 6.5.5 in the book : The Mechanics of Solder Alloy Wetting &
Spreading, ISBN 0-442-01752-9. Several very controlled experiments have
been conducted by Dr. Tench showing what happens with the Cu3Sn and Cu6Sn5
IMCs.  The data shows that the Cu3Sn oxidizes in only 10 minutes and is
very unsolderable. Also check out the information in Soldering In
Electronics, Klein Wassink, ISBN0-901150-14-2, section 4.2.5.3 which
discusses oxidation and Cu/Sn IMCs. The key looks to be which intermetallic
is present - a good deal of the published data I have been reading defines
the "bad" IMC as the Cu3Sn. The consensus trends to the Cu6Sn5 IMC as the
IMC the fluxes can deal with. The SERA testing I have participated in also
trends the same direction. Did you identify the which of the Cu/Sn IMCs
were on your samples? If the IMC was Cu6Sn5 then that would fit the
literature trend. George's ideal of the diffusion kinetics is another
possible detail which may play a part - I am pretty well versed in Sn
oxidation because of my master thesis but the kinetics of copper/tin I need
to do some reading. One interesting point from George's idea - Sn
preferentially oxidizes at the expense of Pb on a tin/lead surface so I
would guess that the copper/tin diffusion kinetics are playing a role too.
Take a look at those references and let me know what you think - oxidation
and IMCs - wonderful discussion topics.

Dave Hillman
Rockwell Collins
[log in to unmask]





Eric Dawson <[log in to unmask]>@ipc.org> on 11/14/2001 02:59:20 AM

Please respond to "TechNet E-Mail Forum." <[log in to unmask]>

Sent by:  TechNet <[log in to unmask]>


To:   [log in to unmask]
cc:

Subject:  Re: [TN] Intermetallic Layers


Hi George,
One pertinent point here is that the intermetallic layers are compounds not
alloys. Thus their oxidising and other chemical reactions will probably be
different from those of their constituent metals.
The surface activation energies may be the key, can you give me references
please George? I would like to follow them up. (See my other reply!)
One point though, I would expect the copper rich compound to lie adjacent
to
the copper interface and the copper deficient one next to the solder
interface. My microsections after solder etching showed that the normally
visible two layers were still present, so I must have been soldering the
copper deficient layer, which, as you say, is the easiest one to solder.
Also, since the melting points of these compounds are higher than soldering
temperatures we would always be soldering to the copper deficient layer. Or
are we? So, open question, can the copper deficient, aka easily solderable,
compound turn into a copper rich layer. Has anybody reading this discussion
got access to a well equipped laboratory?
Regards
Eric Dawson
> -----Original Message-----
> From: Franck, George [SMTP:[log in to unmask]]
> Sent: Tuesday, November 13, 2001 7:20 PM
> To:   [log in to unmask]
> Subject:      Re: [TN] Intermetallic Layers
>
> During my PWB education I learned that there are at least three "alloys"
> of
> copper and tin that are formed as the Copper diffuses into the solder.
> The
> first alloy formed (and I don't remember the ratios) has the highest tin
> to
> copper ratio, and has surface activation energies within the range of
most
> fluxes.  Therefore, this first tin copper alloy, or IMC, is solderable.
> All
> the others alloys, with higher amounts of copper in them,  are not.
>
> Activation energies reflect how strongly attached the Oxygen atom are on
> the
> surface of the metal.  The more copper on the surface alloy, the tighter
> the
> oxygen is attached, the stronger the flux needed to break the oxygen from
> the surface.
>
> While the copper is diffusing into the Solder, the Tin is also diffusing
> into the copper surface, lowering the % tin in the solder alloy, which
> raises the melt temperature of the remaining solder.  It is all quite an
> interesting solid state diffusion system.  By the way, for all intents
and
> purposes, the lead is just too big (physical size of the atom) to
> participate in this diffusion system much, except to get in the way.
>
> It is possible that Eric only exposed the "solderable" tin-copper
> intermetallic in his tests, i.e. the one with the least amount of copper
> in
> it.
>
> What was the magic chemical I played with in my old PWB shop to make
> boards
> solderable, Thiourea hydrochloride?  Wasn't that the active chemical in
> Tarnex also?
>
> George Franck, CID+
> who recalls his "PWB as Black Magic" roots.
>
> --------------------
> Disclaimers:
> 1) If Dave Hillman says I am wrong, then I probably am.
> 2) My company will neither confirm nor deny the existence of any of my
> opinions.
> 3) Tin-copper alloys are commonly referred to as Bronze.
>
> -----Original Message-----
> From: David Hillman [mailto:[log in to unmask]]
> Sent: Tuesday, November 13, 2001 12:25 PM
> To: [log in to unmask]
> Subject: Re: [TN] Intermetallic Layers
>
>
> Hi Eric! Sorry but I humbly disagree. There is an abundance of published
> industry data which shows that oxidized Sn/Cu intermetallic is one of the
> more unsolderable surfaces encountered on an assembly. Problems with poor
> plated thru hole fill due to "weak knees" (thin solder causes the  Sn/Cu
> intermetallic at the hole rim to become oxidized) and thin HASL coatings
> are just two examples of everyday industry solderability issues
associated
> with Sn/Cu IMCs. What type of flux did you use in your testing? Very
> aggressive flux chemistries will allow the soldering of Sn/Cu IMCs but a
> fair majority of the industry is moving away from these types of flux
> formulations. With all that being said, without the Sn/Cu IMC we would
> have
> no solder joints so it is a critical part of a solder joint.
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]
>
>
>
>
> Eric Dawson <[log in to unmask]>@ipc.org> on 11/12/2001 07:49:56 AM
>
> Please respond to "TechNet E-Mail Forum." <[log in to unmask]>
>
> Sent by:  TechNet <[log in to unmask]>
>
>
> To:   [log in to unmask]
> cc:
>
> Subject:  [TN] Intermetallic Layers
>
>
> Hi All,
>
> I notice that a few new references have been made to the above subject
and
> thought I would share some of my early work with you.
>
> In my first post as a graduate, I researched the causes of dewetting on
> circuit boards. I came across a solution, the make-up of which I have
> since
> lost, which dissolved the tin lead alloy but left the two intermetallic
> layers.
>
> I produced a number of one inch square coupons which I soldered using
> 63/37
> alloy, RMA flux and a Tri Moore Rotary Dip Tester.
>
> These were divided into three categories:
>
> 1       Control
> 2       Remove tin lead and re test in the Rotary Dip.
> 3       Remove tin lead, Several hours steam ageing and re test.
>
> Microsections showed that I had taken off the alloy successfully and left
> the IMC.s.
>
> All of the re tested coupons soldered successfully, including the steam
> aged
> ones.
>
> This was some years ago so I cannot remember the etchant nor the hours
and
> conditions in the steam ageing equipment. I do remember that the IMC
> soldered very well so I am always dubious when somebody blames the
> intermetallic for poor soldering.
>
> I seem to be alone in my faith that the IMC solders but this was the
> result
> of my very own work and I stand by it.
>
> Regards
> Eric Dawson, Defender of the IMC.
>
>
--------------------------------------------------------------------------
> --
> -----
>
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases
>
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
>
--------------------------------------------------------------------------
> --
> -----
>
>
--------------------------------------------------------------------------
> --
> -----
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases
>
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
>
--------------------------------------------------------------------------
> --
> -----
>
>
--------------------------------------------------------------------------
> -------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases
>
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
>
--------------------------------------------------------------------------
> -------

---------------------------------------------------------------------------------

Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2