Charles,
In my experience, copper-tin IMCs are normally 1-2 um (40-80 uin) thick after HASL. The rule of thumb
minimum solder coating thickness is 300 uin (0.3 mils) for a 1 year shelf life. This minimum was based on
extensive aging studies of solder coatings by Tin Research Institute (many years ago).
Hope this helps.
Ed Hare
--
SEM Lab, Inc.
Scanning Electron Microscopy and Failure Analysis
Snohomish, WA
(425)335-4400
http://www.sem-lab.com
Charles Barker wrote:
> I am getting differing information from different suppliers of PWB's with
> regard to solder thickness requirements after HASL. Some say 100 to 500
> u-inches, others say 500-800 u-inches and yet others say 1200-3000 u-inches
> (.0012" to .003"). We are looking for 6 months to one year of solderability
> with storage being in an air-conditioned environment with well less than
> saturation humidity in the stockroom. (Generally temp is in the 70 to 75
> deg F range, relative humidity 50 percentish +/- 10 percentage points.)
>
> Can some one tell me what the height of the "normal" intermetallics is on a
> HASLed SMT pad and how much additional solder coating is needed to prevent
> deterioration of the solderability of the pads?
>
> Thanks all,
>
> Charlie B.
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
> ################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|