Hi, FYI
Alvin
Engelmaier wrote:
>
> Hi Mike,
> There is no test method for HASL solder thickness nor is there a general
> specification for a minimum thickness—and perhaps there should not be. The
> minimum solder thickness that will assure solderability will depend on the
> time between the HASL-process and the reflowing of the assembled PCB, because
> thin solder coatings have a limited shelf life which is also temperature-
> dependent. This comes from the fact that the intermetallic compound (IMC)
> layer Cu6Sn5 will grow and thus consume the available tin. This diffusion
> process is temperature-dependent. As the tin is consumed, the layer above the
> IMC layer becomes increasingly lead-rich and therefore there will be an
> increase in the Liquidus temperature making subsequent reflow soldering more
> difficult if not much original near-eutectic solder remains above it. In the
> worst case, the IMC can grow to the surface—upon exposure to oxygen the
> formerly solderable IMC becomes non-solderable.
> So, you have to judge for yourself, what minimum solder thickness is
> appropriate for your needs. Anything less than 2 micrometers has a rather
> limited shelf life, while above 5 micrometers a long shelf life for most
> reasonable storage conditions is assured.
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
################################################################
|
|
|