TECHNET Archives

June 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Date:
Wed, 24 Jun 2009 07:59:33 -0700
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, John Burke <[log in to unmask]>
Subject:
From:
John Burke <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (87 lines)
Ugh,

Last time I saw something like that was on a wave solder machine where the
solder pump impeller was breaking up which lead to a very "rough" looking
joint with traces of iron.

John Burke
(408) 515 4992

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Wednesday, June 24, 2009 6:41 AM
To: [log in to unmask]
Subject: Re: [TN] SN100C I don't like the look of board pads

Morning Inge and Everybody!

Got your pics posted Inge, and as usual, your pictures always give me a
new window in which to see things. Here they are:

http://stevezeva.homestead.com/files/SN100CSEM1.jpg

http://stevezeva.homestead.com/files/SN100CSEM2.jpg

I renamed your files and saved them as *.jpg files because my web page
doesn't allow me to use *.tif files. We've only used SN100 here a few
times, and you're right, ours looked just like regular 63/37 HASL. We've
never had a SEM done on the boards we used, so I have nothing to compare
your images to. But the boards we used were nice and shiny.

Steve

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
Sent: Wednesday, June 24, 2009 7:55 AM
To: [log in to unmask]
Subject: [TN] SN100C I don't like the look of board pads

 Hi all,
 
will send pictures to Steve.
The two SEM images show SN100C boards that we got recently.
I don't like the look of the solder surface. Very grainy and with lots
of copper (darker spots). EDAX gives even fragments of iron. My first
thought was that the manufacturer had contaminated baths, which will be
denied, of course. Anyway, my opinion is, that SN100C should be more
like ordinary tin/lead, i.e nearly zero copper and a more shiny
approach. 

/Inge
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest