TECHNET Archives

October 2013

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Steve Gregory <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Date:
Thu, 10 Oct 2013 15:18:34 -0600
Content-Type:
text/plain
Parts/Attachments:
text/plain (75 lines)
Hey Ed,

Haven't run across that problem (yet), and don't really know how to
clean that. But I did run across another brand of spacers that I didn't
know about before that's made of different material than what Bivar
dissolvable spacers are made of...aren't bivar spacers made of some sort
of sugar ? 

http://www.multi-seals.com/washawayspacers.php

They're made of something called Polyvinylpyrrolidone, and  contain no
ionizable material, salts, sugars, metals, or soaps, and they are
non-corrosive, non-conductive, and non-toxic.

I just found them in a search today. I'm getting a sample pack of them
sent to me check them out myself, you might check them out too if you've
never tried them. 

Steve 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ed Popielarski
Sent: Thursday, October 10, 2013 2:31 PM
To: [log in to unmask]
Subject: [TN] Charred dissopad residue

Hi all,

Had an odd problem today.

We have built many of these assemblies with tin/lead solder but just now
switched to lead free solder (higher temperature).

The "Dissopad" contacting the PCB (at a via) liquefied, spread and
charred. The residue is very difficult to remove, especially a concern
since it is under components and could be "conductive". (pix available
on request)

We tried cleaning this with isopropyl alcohol and it didn't seem to
dissolve the charred residue at all.

I soaked one PCB in 140F DI water for 30 min. and re-cleaned in the
aqueous cleaner. It did seem to remove the heavier residue, but there
remains a film and smaller clumps on the board surface.

Any suggestions would be appreciated!


Ed Popielarski
Engineering Manager

[Description: FullLogo]
                               970 NE 21st Ct.
                              Oak Harbor, Wa. 98277

                              Ph: 360-675-1322
                              Fx: 206-624-0965
                              Cl: 949-581-6601

https://maps.google.com/maps/myplaces?hl=en&ll=48.315753,-122.643578&spn
=0.011188,0.033023&ctz=420&t=m&z=16&iwloc=A


______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2