> We are looking for the IPC spec that calls out the maximum Au plating
> thickness on leads in order to prevent Au embrittlement.
>
> Hi Karen,
No such thing.
Reason, Au-embrittlement depends on too many variables. A 4 wt.% Au of
uniform distribution is the VERY APPROXIMATE 'red flag' threshold. If you have
non-uiform distribution—the more likely scenario-- lower Au % can lead to
Au-embrittlement.
Werner
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------