Yes we have. Here are some of our findings.
*Usually due to excessive change in temperature
- Reflow, cleaning, wave solder, rework
- Inability of capacitor to relieve stresses during transient conditions.
* Maximum tensile stress occurs near end of termination
- Determined through transient thermal analyses
- Model results validated through sectioning of ceramic capacitors exposed
to thermal shock conditions
* Three manifestations
- Visually detectable (rare)
- Electrically detectable
- Microcrack (worst-case)
*Variations in voltage or temperature will drive crack propagation
* Induces a different failure mode
- Increase in electrical resistance or decrease capacitance
Corrective Actions (Manufacturing)
* Solder Reflow
- Room temperature to preheat (max. 2-3oC/sec.)
- Preheat to at least 150oC
- Preheat to maximum temperature (max. 4-5oC/sec.)
- Cooling (max. 2-3oC/sec.)
- - In conflict with profile from J-STD-020C (6oC/sec.)
- Make sure assembly is less than 60oC before cleaning
* Wave soldering
- Maintain belt speeds to a maximum of 1.2 to 1.5 meters/minute
* Touch Up
- Eliminate
Corrective Actions (Design)
* Orient terminations parallel to wave solder
* Avoid certain dimensions and materials (wave
soldering)
- Maximum case size for SnPb: 1210
- Maximum case size for SAC: 0805
- Maximum thickness: 1.2 mm
- C0G, X7R preferred
* Adequate spacing from hand soldering operations
* Use manufacturer's recommended bond pad dimensions or smaller (wave
soldering)
* Smaller bond pads reduce rate of thermal transfer
Cracking parallel to the electrodes is due to stackup or sintering processes
during capacitor manufacturing
* These defects can not be detected using in-circuit (ICT) or functional
test
- Requires scanning acoustic microscopy (SAM)
* With poor adhesion, maximum stress shifts away from the termination to the
defect site
* No correlation between failure rate and cooling rates (0.5 to 15C/sec)
Flex Cracking of Ceramic Capacitors
*Excessive flexure of PCB under ceramic chip capacitor can induce cracking
at the terminations
* Pb-free more resistant to flex cracking
- Correlates with Kemet results (CARTS 2005)
* Rationale
- Smaller solder joints
- Residual compressive stresses
- Influence of bond pad
* Action Items
- None
Clayton Bonn
Reliability Resources/DfR Solutions
Ph: 714-903-1005
Cell: 714-612-9359
e-mail:[log in to unmask]
www.reliability-resources.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Igoshev, Vladimir
Sent: Monday, July 14, 2008 6:08 AM
To: [log in to unmask]
Subject: [TN] Ceramic caps
Hi TechNeters,
I came across an unusual (at least to me) failure mode of ceramic caps.
They crack along the component body in either normal (from top all the
way through to the bottom), or parallel (from one side all the way
through to the other side) direction to the board the caps are mounted
on.
Has anyone seen something similar?
Thanks a lot in advance.
Regards,
Vladimir
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|