Russ
SnPb HASL soldered with SnAgCu works fine. At least it alloys. The Pb
is found as contamination in the intermetallics between the Sn dendrites
of the Pb free solder. We are right now analysing samples. What we found
is that the Pb doesn't occur pure but forms an alloy with the silver of
the solder. The whole thing becomes somewhat complicated since
intermetallic SnAgPb and AgCuPb phases occur that are not found in the
literature. However, fascinating metallurgy.
Best regards
Guenter
EMPA
Swiss Federal Laboratories for Materials Testing and Research
Centre for Reliability
Guenter Grossmann, Senior Engineer
8600 Duebendorf
Switzerland
Phone: xx41 1 823 4279
Fax : xx41 1 823 4054
mail: [log in to unmask]
>>> [log in to unmask] 30.03.2005 14:19:16 >>>
Good Morning Technet,
I am at the early stages of learning about lead free solder as an
alternative option to our current tin/lead solder HASL.
Is there anyone out there who can comment about their experiences?
Currently I have no customers requesting this process, but I need to
be
ahead of this need when feasible.
Vendors have provided both sides, yes PCB makers are doing it and a
large
PCB maker tried it and discontinued using it.
Thanks in advance.
Russ Burdick, trying to lessen the HASL hassle
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|