TECHNET Archives

October 2012

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Gumpert, Ben" <[log in to unmask]>
Date:
Thu, 4 Oct 2012 10:36:20 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
Douglas Pauls <[log in to unmask]>
Message-ID:
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (195 lines)
Ben,
It might be the brushes themselves.  Many brushes are shipped with a mild 
wax on the bristles to help them keep the shape during shipping.  We 
always require our operators to solvent clean the bristles on new brushes 
before their first use.

Doug Pauls



From:   "Gumpert, Ben" <[log in to unmask]>
To:     <[log in to unmask]>
Date:   10/04/2012 10:26 AM
Subject:        Re: [TN] EXTERNAL: Re: [TN] UV40 Conformal Coating
Sent by:        TechNet <[log in to unmask]>



Lee,

Our preferred method of application is automated spray, we are just 
performing some initial testing with brush application.

Do you expect that I'll see a dramatic difference between the two 
applications? I typically do with a solvent based coating, since the spray 
process results in the loss of solvents, but with this material I'm not 
sure that there will be much change.

Ben

-----Original Message-----
From: lee Hitchens [mailto:[log in to unmask]] 
Sent: Thursday, October 04, 2012 7:57 AM
To: 'TechNet E-Mail Forum'; Gumpert, Ben
Subject: RE: [TN] EXTERNAL: Re: [TN] UV40 Conformal Coating

Hi Phil

Is this going to be your preferred application method or are you just 
evaluating it with the brush for initial trials?

Best Regards

Lee Hitchens
Technical Director

SCH Technologies is a Division of SCH Services Limited
Mob: +44 (0) 7862 25 33 21 www.conformalcoating.co.uk

TECHNICAL SUPPORT SERVICE
 
SCH Services Ltd offers a Technical Support Helpline to help address all 
issues relating to reliability. This includes contamination testing, 
cleanliness and cleaning issues, plus any coating related questions.
Please contact us via email or telephone:
 
[log in to unmask]   +44 (0)1226 249019 (office hours & answerphone)   
+44
(0)7862 253321 (out-of-hours emergency)

The opinions expressed in this e-mail are strictly those of the sender and 
not of SCH Services Limited. This communication may contain information 
which is confidential and may also be privileged. It is for the exclusive 
use of the intended recipient(s). Unauthorised use, copying or disclosure 
of any of it may be unlawful. If you are not the intended recipient(s) 
please note that any distribution, copying or use of this communication or 
the information in it is strictly prohibited. If you have received this 
communication in error please notify us by e-mail or by telephone (+44
(0)1226 249019) and then delete the e-mail and any copies of it. Virus 
Warning - Although steps have been taken to ensure that all email and 
attachments are virus-free, we cannot guarantee nor be held liable.
 
Company Registration: 04043334
Registered office: SCH Services Limited Newburgh Building McLintock Way 
Barnsley South Yorkshire S70 6BF



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Gumpert, Ben
Sent: 04 October 2012 12:46
To: [log in to unmask]
Subject: Re: [TN] EXTERNAL: Re: [TN] UV40 Conformal Coating

Lee, Phil,

I typically use urethane coating, so I am used to something that thickens 
up during application, so this is certainly different than what I am used 
to.

What I've tried so far is hand application using a brush, and I see the 
dewetting happening on vertical lead areas, like the legs of gull-wings. 
And it's happening almost right away, before I go to cure.

I'm using some dummy test boards, but they've been through an in-line 
cleaner (Kyzen A4625) post soldering, and a hand clean with IPA just prior 
to coating.

Ben

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Phil Kinner
Sent: Wednesday, October 03, 2012 5:10 PM
To: [log in to unmask]
Subject: EXTERNAL: Re: [TN] UV40 Conformal Coating

Hi Ben,

How are you applying the material and what components are you seeing this 
on? 

There are some application tricks to the trade to minimize this 
phenomenon.... You can contact me offline if you'd like to discuss this 
further.

Otherwise, I'd recommend you speak to  both Matt Eveline at HumiSeal and 
Jon Urquhart at PVA, both great resources to get you going in the right 
direction.

Best Regards,

Phil
+44 7703 795422

Sent from my iPhone

On 3 Oct 2012, at 22:47, Lee Hitchens <[log in to unmask]> 
wrote:

> Hi Ben what are you comparing too? A solvent based coating or 
> something
else! Is the coating running during or just after application or during 
the cure process under the uv lights where it can get hot? 
> 
> Best regards
> 
> Lee hitchens
> 
> Sent from my iPad
> 
> On 3 Oct 2012, at 21:39, "Gumpert, Ben" <[log in to unmask]> wrote:
> 
>> Technetters,
>> 
>> I'm evaluating Humiseal's UV40 conformal coating, but I'm seeing 
>> wetting
issues - where the coating completely runs off of vertical lead surfaces.
>> 
>> I see from some e-mails a couple of years ago that some of you are 
>> using
this coating material, or were looking into it. Is anyone else seeing this 
problem, or have some suggestions to fix?
>> 
>> Ben
>> 
>> 
>> _____________________________________________________________________
>> _ This email has been scanned by the Symantec Email Security.cloud 
>> service.
>> For more information please contact helpdesk at x2960 or 
>> [log in to unmask] 
>> _____________________________________________________________________
>> _
> 
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud 
service.
> For more information please contact helpdesk at x2960 or 
> [log in to unmask] 
> ______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________


______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________




______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2