Purple discoloration on gold plated boards is due to the formation of
'purple of Cassius', which yu should be able to find out about in your
chemistry books. I believe that it is due to some contamination absorbed
into the resin of the laminate. I remember this problem 15 years ago,
and a change of laminate supplier had the problem go away.

Dougal
Dougal Stewart
Product Development Manager
Viasystems Selkirk Ltd
Selkirk, Scotland, TD7 5EJ
Tel: +44 1750 21601
Fax:+44 1750 22513
email   [log in to unmask]

> -----Original Message-----
> From: [log in to unmask] [SMTP:[log in to unmask]]
> Sent: Tuesday, May 19, 1998 7:00 AM
> To:   [log in to unmask]
> Subject:      [TN] DISCOLORATION
>
> HI ! EVERYBODY
> I HAVE A PROBLEM.
> AFTER I/R REFLOW PROCESS, PCB WAS DISCOLORED AROUND
> GOLD PLATING, ESPECIALLY EXPOSED EPOXY AREA CHANGED
> LIGHT VIOLET.
> THE PCB WAS APPLIED A HASL PROCESS AND EDGE CONNECTOR
> GOLD PLATING. WE TESTED MANY TIMES AND ONLY PCB WHICH
> WAS APPLIED THE HASL PROCESS AND GOLD PLATING PROCESS.
>
> THERE IS LOW PEAK OF Sn BY SEM ANALYSIS ON THE DISCOLORED
> SPECIMEN ONLY.
>
> THE GOLD PLATING CHEMICAL MAKER SAID :
> IF AMINO-COMPOUNDS WHICH IS USED HARDNER OF EPOXY
> MATERIAL JOIN WITH A CYANIDE, PCB CAN DISCOLORATION AFTER
> THERMAL SHOCK.
>
> PLEASE HELP ME WHY THE PCB WAS DISCOLORED AS SOON AS
> POSSIBLE.
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV
> 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in the body:
> To subscribe:   SUBSCRIBE TechNet <your full name>
> To unsubscribe:   SIGNOFF TechNet
> ################################################################
> Please visit IPC web site (http://jefry.ipc.org/forum.htm) for
> additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or
> 847-509-9700 ext.312
> ################################################################

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################


ATOM RSS1 RSS2