TECHNET Archives

March 2007

TechNet@IPC.ORG

Options: Use Proportional Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Inge <[log in to unmask]>
Date:
Mon, 19 Mar 2007 18:46:38 +0100
Content-Type:
text/plain
Parts/Attachments:
text/plain (67 lines)
Yep, as would say your gran-granfather.
Inge

----- Original Message ----- 
From: "John Maxwell" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Monday, March 19, 2007 5:06 PM
Subject: Re: [TN] "Greenish colour on traces"


> Ingemar,
> We must also remember that nickel is  magnetic as well increasing its 
> impedance at high frequencies. That is a reason that many GHz passive 
> components do not use a nickel barrier on their terminations.
>
> John maxwell
>
>
>>That's something else! You did not tell what purpose. It's right, for
>>some multiGHZ bands, where low losses are wanted, we don't use nickel
>>plating because it's higher resistivity. Some nickel platings can have
>>10 times higher losses than Copper and Gold! In these cases, we use just
>>copper (no plating at all)if it's possible in environmental point of
>>view, or we use tinned copper lines. So, silver over copper is
>>theoretically right. And metallurgically spoken, silver on copper has
>>been used for centuries. What I don't understand is why add gold. Maybe
>>to avoid silver tarnish, if the package is not hermetic.
>>Resistivity microOhm x cm :
>>
>>Electronic solder       17-20
>>Pure Tin                9-11
>>Electroless nickel      50-100
>>Electrolytic nickel      8-10
>>Electrolytic Gold        2.5
>>Copper lines             1.8
>>Electrolytic Silver      1.6
>>
>>When you look at the above table, you will understand why Silver.
>>
>>Inge
>>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
> for additional information, or contact Keach Sasamori at [log in to unmask] or 
> 847-615-7100 ext.2815
> -----------------------------------------------------
> 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2