It sure sounds you are describing what is called black pad nickel.  The
black nickel/gold interface has very poor adhesion properties.  I would bet
any nickel residues were from process chemistry being trapped between the
poorly adherent gold and the black pad surface.    I mid phos nickel would
have good corrosion resistance to steam (water) and would not be corroded in
humidity testing due to lack of gold.  Lack of gold would simply cause poor
solderability.

You should read and article in January Circuitry Magazine called
"Electroless Nickel Immersion Gold and Black Pad".  I can send you a copy of
the article, if you do not get the magazine. Just send me an email request.

Best Regards,
Rob Durante
[log in to unmask]

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Gregg Klawson
Sent: Wednesday, January 31, 2001 6:07 AM
To: [log in to unmask]
Subject: [TN] ENIG moisture reisistance - Ni corrosion

We have just run several ENIG finished board assemblies through a 10 day
cycled system-level humidity test for the first time.  Our previous
experience base has been with HASL'd and/or conformal coated boards.  Two
issues have come up which we don't fully understand.

The first issue is that the boards have a light green to white translucent
residue areas which have formed on top of the Au surfaces which were not
soldered (via-hole lands).  SEM-EDS and FTIR shows these residues contain
water and nickel species, perhaps a nickel sulfate or carbonate.  Taking a
cotton swab with IPA and gently rubbing the residues causes small pieces of
Au to flake off revealing a dark surface (perhaps black).  It appears that
there was a pin hole in the gold and the underlying nickel corroded
producing the residue and corroding underneath the "good" gold area.

I'm wondering if this corrosion is "normal" for ENIG finished boards in
this type of environment?  Or do we potentially have some other
issue?   Any reliability concerns?  All the PWBs were built in the same
shop at different times.

Thanks in advance for your comments.  Second issue coming up in a separate
email to Technet.

Best regards,
Gregg Klawson
General Dynamics Communication Systems
Taunton, Massachusetts, USA
mailto:[log in to unmask]

The views expressed are the author's and do not necessarily reflect the
official position of General Dynamics or any of its subsidiaries.

----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2