30 micro inches of gold cannot be achieved through ENIG plating. From
Coombs' Printed Circuits Handbook;
"In this finish a layer of electroless nickel with a thickness of 120 to 240
micro inches is deposited on the copper surface. This is then followed by a
thin coating (2-4 micro inches) of immersion gold. The nickel is a diffusion
barrier to copper and is the surface to which the soldering occurs. The
function of the immersion gold is to protect the nickel from oxidation or
passivation during storage."
Your specifications would require gold electroplate. The nickel thickness
seems to be an order of magnitude too thin. 200-300 micro inches nickel
plated with 30 micro inches of gold would seem to be a compromised gold
thickness intended to have reasonable wear resistance and still allow for
acceptable soldering process results.
A word of caution. The gold would be too thick for most solder paste -
surface mount applications, resulting in brittle solder connections. We
worked out a rule of thumb some months ago, here on the TechNet. I think the
number was 5 mil stencil - 10 micro inches max gold thickness. I am sure the
thread is in the archives.
This causes some problems in practice because it is difficult to protect the
nickel with a 10 micro inch max on gold electroplate. It is a process thing.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David Harman
Sent: Friday, December 29, 2006 1:09 AM
To: [log in to unmask]
Subject: [TN] Questions on ENIG VS gold plating
I need some help in understanding.
Are specified requirements are emersion gold plate per
Mil-G-45204 type 2, gold plating thickness maximum of .00003 inches (30
micro inches) over minimum of .00005 inches (50 micro inches) nickel for our
PCB
Is this a standard that is used widely, any other recommendations?
My supplier has indicated the following.
The specifications you listed in your e-mail do not apply to the ENIG finish
(Immersion Gold, electroless nickel)
Mil -G- 45204 refers to Electroplated Gold, Type 2 is 99.0% purity
IPC 6012B Table 3-2 requirements for ENIG are 1.97 u" minimum immersion gold
and 118 u" minimum of electroless nickel.
Which is a better specification? What would give better quality /
reliability? Is there anyway to correlate the two different specifications.
Can I correlate ENIG specs, to that of gold plating.?
Dave
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|