TECHNET Archives

November 2005

TechNet@IPC.ORG

Options: Use Proportional Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Ofer Cohen <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Ofer Cohen <[log in to unmask]>
Date:
Fri, 11 Nov 2005 11:37:38 +0200
Content-Type:
text/plain
Parts/Attachments:
text/plain (103 lines)
Willis,
Welcome to the black group of the black pads. We've experienced the phenomena lately. The balls were left on the PCB, while the BGA, leg-less, fell off after the soldering. Failure analysis showed clearly balck pads phenomena on the BGA substrate.

Ofer Cohen
Siemens

> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of WTSJ-Willis Tam
> Sent: Friday, November 11, 2005 08:31
> To: [log in to unmask]
> Subject: [TN] urgent issue BGA fall out
> Importance: High
> 
> > Dear All,
> > 
> > Recently, we found a very strange defect with the BGA IC.
> > 
> > Here's our process flow:  SMT---> De-panel (by V-cut machine)---> 
> > Functional test--->final inspection
> > 
> > We found around 10 pcs BGA falling out either at the process of 
> > de-panel or functional test, defect rate less than 0.1%. The defect 
> > only happened in 2 days, It's very strange, all the solder 
> balls adhere to PCB. there's no
> > solder ball adhere to the BGA substrate.   
> > 
> > Investigations from our side:
> > 1. We have been built the same product since April 2004. no 
> issue before.
> > 2. Since May 2005, the SMT process was converted to RoHS, 
> BGA also has 
> > been changed to green type since then, monthly output around 200K.
> > 3. The BGAs were 100% baked under 110 degreeC for 24 hrs before SMT.
> > 4. We use Loctite LF318 solder paste for SMT, the time between 70 
> > degreeC to peak 245 degreec is around 250 seconds.
> > 5. The BGA only subjected to 1 time reflow (only 1 side with 
> > components) 6, We have reflow fixture to support the board during 
> > reflow. there's no warpage issue.
> > 7, Use Vcut machine to separate the units from a 6 up-panel PCB, no 
> > extra stress to the board.
> > 8. Use pogo pin to make connection for functional test fixture, no 
> > extra stress.
> > 
> > Information of BGA.
> > 1. It's a solder mask defined substrate. with ENIG surface 
> finishes. 
> > 2. 0.8mm pitch, pad size 0.35mm.
> > 3. IC supplier apply solder ball with flux only, without 
> solder paste.
> > 
> > Would anybody give me some advices, what shall be the most possible 
> > root cause? it's a BGA IC issue or a SMT process issue? How 
> to improve?
> > 
> > 
> > Thanks
> > Willis Tam
> > 
> > 
> > 
> > 
> > 
> > 
> > 
> > 
> >  
> > 
> > 
> > 
> > 
> > 
> > 
> > 
> > 
> > 
> > 
> 
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 
> 1.8e To unsubscribe, send a message to [log in to unmask] with 
> following text in the BODY (NOT the subject field): SIGNOFF 
> Technet To temporarily halt or (re-start) delivery of Technet 
> send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) 
> To receive ONE mailing per day of all the posts: send e-mail 
> to [log in to unmask]: SET Technet Digest Search the archives 
> of previous posts at: http://listserv.ipc.org/archives Please 
> visit IPC web site 
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for 
> additional information, or contact Keach Sasamori at 
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
> 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2