The mechanical stress comes at low temperatures, after curing the coating,
not at elevated temperatures. From our experience, if using hard conformal
coatings like urethane, use of protective sleeving can be avoided if the
coating fillet at the base of the component is less than 0.012" high
(measured from the board surface)
R. G. Blomberg
Honeywell - Space Systems
Staff Production Engineer
(727) 539-5534 voice
727-539-4469 Fax
[log in to unmask]
-----Original Message-----
From: Roberts Jon [mailto:[log in to unmask]]
Sent: Wednesday, August 30, 2000 3:20 PM
To: [log in to unmask]
Subject: Re: [TN] Glass component on trace
The only thing comes to mind if you are to conformal coat the board then you
might have to put sleeving over the diode. This is to protect it from
mechanical stress as the conformal coating cures because the board and glass
diode are expanding at different rates. There has been experience with
diodes cracking. I think even after the cure this can be a problem with the
environment the assembly will experience. I have always wonder if any
problem can occur from bonding diodes to the board on the bottom of boards
and running them through the wave. I think there is something in the
Handbook for J-Std-001 about this. Jon
-----Original Message-----
From: Jan Satterfield [mailto:[log in to unmask]]
Sent: Wednesday, August 30, 2000 1:21 PM
To: [log in to unmask]
Subject: [TN] Glass component on trace
I have a pwb that does not have solder mask on it. We are mounting a glass
diode with the body directly on top of a .065 trace. The drawing does not
call out for sleeving and there is nothing in IPC-610 which addresses this.
It just doesn't feel right to me....flashbacks of WS 6536 perhaps. Should
this be of any concern????
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|