TECHNET Archives

July 2006

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
"David D. Hillman" <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Thu, 20 Jul 2006 07:25:51 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (162 lines)
Hi folks! One other fact to consider is that the formation of silver
sulfide will cause a significant increase in the contact resistance. I
can't seem to find the typical contact resistance value in my database (its
in there somewhere) but I'll keep looking. Silver oxide is as conductive as
elemental silver and silver chlorides only increase the contact resistance
values minimally. Leo - an immersion silver finish that has silver sulfide
on its surface would look black/dark blue/purple visually. Yellow or light
brown would indicate either chlorides or a small amount of silver sulfide.
Good luck.

Dave Hillman
Rockwell Collins
[log in to unmask]




             John Burke
             <[log in to unmask]
             >                                                          To
             Sent by: TechNet          [log in to unmask]
             <[log in to unmask]>                                          cc

                                                                   Subject
             07/19/2006 11:25          Re: [TN] Immersion Silver for ICT
             AM


             Please respond to
              TechNet E-Mail
                   Forum
             <[log in to unmask]>
             ; Please respond
                    to
                John Burke
             <[log in to unmask]
                     >






Me too,

I know that silver oxide is conductive, but I do not think that the
sulphides are.

I have always printed them with solder to avoid cosmetic problems
downstream, and also as a wear surface where card guides are a factor and
the contact is used as an EMI earthing point, although in this latter
instance it is wise to break up the earthing card guide edge ground into a
dot pattern and cover the rest with solder resist.

John

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Darrel Therriault
Sent: Wednesday, July 19, 2006 8:57 AM
To: [log in to unmask]
Subject: Re: [TN] Immersion Silver for ICT

Leo,

I always included test pads in my solder stencil so they would be
soldered.

DJT



Lin Leo <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
07/19/2006 12:04 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Lin Leo <[log in to unmask]>


To
[log in to unmask]
cc

Subject
[TN] Immersion Silver for ICT






Hi,

  Recently, I met a customer complaint for Immersion Ag boards.  Immersion
Ag  boards in assembly side weren't applied solder on ICT(in circuit test)
pads.  After assembly, Ag surface discoloration problem and ICT failure
defect were found in those pads.  Those pad were still solderable.  ICT
was OK after soldering.  Does anyone have similar experience?  How can I
solve this problem?  Does it need to suggest pre-solder before ICT?  It's
chronic or excursion issue for immersion Ag surface finish?

  Best regards

  Leo

 ___________________________________________________
 ??? Yahoo!?????? 7.0???????????

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
 http://messenger.yahoo.com.tw/


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2