TECHNET Archives

April 1998

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
Subject:
From:
Paul Gould <[log in to unmask]>
Date:
Tue, 28 Apr 1998 08:59:35 +0100
In-Reply-To:
<F9C0B6DC6BA9D111AC3F00A0C95B46C2846C2D@FMSMSX39>
MIME-Version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Paul Gould <[log in to unmask]>
Parts/Attachments:
text/plain (33 lines)
Olson, Jack C wrote:-
>I was under the impression that black oxide provided more "tooth" for
>bonding copper to the substrate material.  Recently I was told is was just
>to protect the surface during handling. Since I can't find it in Coombs
>Handbook, can anyone briefly explain?
Hi Jack
You are right, the reason for oxide treat of copper foil is to improve
the bond strength. It makes handling more difficult as it is easily
marked. Early oxides were cuprous and readily attacked by acids. They
could also be quite thick and hence led to pink ring phenomenon around
holes. Nowadays the norm is to reduce the oxide coating to cupric by
post treatment. This is impervious to acid attack and is also much
thinner which prevents pink ring formation.
There are alternative finishes but, as far as I know, none of them give
higher bond strengths than reduced oxide.
Paul Gould
[log in to unmask]
Teknacron Circuits Ltd
Fax: 1983 865141
Tel: 1983 866531

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
################################################################


ATOM RSS1 RSS2