TECHNET Archives

September 2013

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Fri, 27 Sep 2013 08:31:08 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Gerry Gagnon <[log in to unmask]>
Message-ID:
Subject:
From:
Gerry Gagnon <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (31 lines)
Glenn,
 
I agree with your assessment in light of the data we have received.
 
For more on item 2, yes, the first thing folks expect is thin silver, which does occur from time to time and the culprit is copper oxide as you state.
 
However, I have seen wild discolorations in areas with silver thickness well within spec, but these were circumstances where the boards received very high amounts of heat in localized areas, particulary along the rails of panelized boards where the rails were silver. When determining reflow parameters, most folks, myself included, do not tend to thermocouple the rails, so they may not know how hot it gets there. I recommend soldermasking the rails.
 
Brs,
 
Gerry Gagnon

 
> Date: Fri, 27 Sep 2013 01:11:56 -0500
> From: [log in to unmask]
> Subject: Re: [TN] Immersion Silver Board Finish Tarnishing
> To: [log in to unmask]
> 
> I see two possibilities:
> (1) the test probes are coated and not making reliable contact.
> (2) If a shading other than silver is observed, it may be that the silver was too thin and the copper migrated to the surface and was oxidized by time or by the processing temperature, if a process was attempted.  I will suspect copper oxide and I would examine some unprocessed bare boards under a microscope looking for signs of visible copper. In three days, even at pre-baking temperatures, you should not have copper oxides on the surface. 
> 
> The silver is a very thin surface protectant (approx. 0.10um) and migrates into the solder when processed. You solder to the copper.
> Glen
 		 	   		  

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2