Hello Jim:
I too would like to have a copy of this chart, if you don't mind.
My fax # is 208-622-4377.
I highly appreciate that.  Thanks and regards.
Gabe Cherian


-----Original Message-----
From: James R. Paulus <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Date: Wednesday, October 21, 1998 8:27 AM
Subject: Re: [TN] FR4 thermal expansion


>I have a comprehensive chart which I can fax you, if you want to provide
the
>phone #.
>Generally, Z-axis is 60 to 80 ppm (or microinches/inch/C), X is 17-20 ppm,
and
>Y is 15 to 18 ppm.  Lots of variables however:
>a.  These values are for a temp ramp up to the Tg, which is 135C typically
for
>FR4.
>b.  Remember that FR4 today can be a material with a Tg as high as 180C.
>Higher Tg FR4's tend to exhibit a slightly lower Z-expansion below the Tg
than
>135C types.
>c.  Z-axis is particularly affected by resin:glass ratio.  Higher Resin
>content means greater expansion, which has to be considered in high layer
>count designs.
>d.  Above the Tg,  the X and Y movements get squirrelly because the
softened
>resin allows the glass fabric to pull back against the expanding matrix,
>resulting in much lower values.
>jimpaulus
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
>To subscribe:   SUBSCRIBE TechNet <your full name>
>To unsubscribe:   SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
>################################################################
>

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################


ATOM RSS1 RSS2