TECHNET Archives

April 2018

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Douglas Pauls <[log in to unmask]>
Date:
Mon, 16 Apr 2018 13:15:17 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Message-ID:
Content-Transfer-Encoding:
quoted-printable
Subject:
From:
Steve Gregory <[log in to unmask]>
X-cc:
TechNet E-Mail Forum <[log in to unmask]>
In-Reply-To:
Content-Type:
text/plain; charset="UTF-8"
MIME-Version:
1.0
Parts/Attachments:
text/plain (201 lines)
Thanks Doug,

That's something that hadn't occurred to me, I was worrying about degrading
the carrier tape/cover film tape so much that it would have problems in the
pick and place machine. So now I'm wondering what the alternative is for
parts that have exceed their floor life while on a reel? Strip them off the
tape, bake them, then re-reel them again? That would be great if we had a
tape and reel machine.

So, based on what Doug says, if you get things hot enough to diffuse the
moisture out of the parts, you are likely doing nasty things to the plastic
carriers to cause them to outgas/offgas stuff out on the parts.

Steve

On Mon, Apr 16, 2018 at 12:25 PM, Douglas Pauls <
[log in to unmask]> wrote:

> Steve,
> I would not be an advocate of this approach.  If you get the tape and reel
> hot enough to make moisture diffuse out, you may also be causing the
> plastic to outgas/offgass materials that would be detrimental to the
> component.
>
>
> Doug Pauls
> Principal Materials and Process Engineer
> Rockwell Collins
>
> On Mon, Apr 16, 2018 at 9:19 AM, Steve Gregory <[log in to unmask]> wrote:
>
>> Hi All,
>>
>> I know this thread is about vacuum baking, but I would like to ask about
>> baking components on tape and reel, I have not actually done this. I
>> remember seeing discussion about the topic on Technet, but I can't
>> remember
>> all the details.
>> I know when I ask what temperature is safe to bake tape and reel
>> components
>> "it depends" will come up, it probably depends on what kind of carrier
>> tape
>> on top film cover tape is used, is it pressure sensitive adhesive or heat
>> seal cover tape? I'm seeing a need that may require more baking of reeled
>> components now for some reason.
>>
>> Is it just me, or does it seem that more and more components are being
>> designated as MSL 2A and higher lately?
>>
>> Steve
>>
>> On Mon, Apr 16, 2018 at 8:09 AM, Yuan-chia Joyce Koo <[log in to unmask]>
>> wrote:
>>
>> > you can make board vertical stand in the PWA carrier tray with slot.
>> you
>> > need surface area for moisture to escape...assume you use low
>> temperature
>> > in vacuum baking, little warpage would happen  unless it is very thin
>> large
>> > size board.
>> > On Apr 16, 2018, at 9:23 AM, Robert Kondner wrote:
>> >
>> > Hi,
>> >>
>> >>  If you have a stack of PCBs, lets say 25 or 50 boards which is a
>> stack 2
>> >> or 3 inches high, can water vapor diffuse out the space between the
>> boards?
>> >> Does laying a thick tissue between the boards help or is it best to
>> place
>> >> each board in edge supported carriers?  I worry about warp if a board
>> is
>> >> edge supported while at elevated temps.
>> >>
>> >> Does anyone has knowledge here or even an educated guess?
>> >>
>> >> Thanks,
>> >> Bob K.
>> >>
>> >> -----Original Message-----
>> >> From: TechNet <[log in to unmask]> On Behalf Of David Hillman
>> >> Sent: Monday, April 16, 2018 8:11 AM
>> >> To: [log in to unmask]
>> >> Subject: Re: [TN] Vacuum Baking
>> >>
>> >> Hi folks - we did some vacuum baking experimentation a few years back
>> and
>> >> yes, vacuum baking can be effective but it is not as straight forward
>> as
>> >> you would imagine. You need to carefully select the vacuum bake
>> parameters
>> >> or you will actually impede water diffusion. You can cause ice
>> formation
>> >> rather than water evaporation depending on your parameters (put a
>> shallow
>> >> pan of water in a vacuum chamber and try it, its kinda fun). Wayne's
>> >> approach is much simpler and far more practical/effective in terms of
>> >> moisture removal.
>> >>
>> >> Dave Hillman
>> >> Rockwell Collins
>> >> [log in to unmask]
>> >>
>> >>
>> >> On Sun, Apr 15, 2018 at 11:43 AM, Wayne Showers <
>> >> [log in to unmask]> wrote:
>> >>
>> >> The problem with vacuum drying is not so much the boiling point of
>> >>> water as in an unimpeded environment, those values are: At 25" Hg :
>> 56C,
>> >>> 27" Hg :
>> >>> 45C, 28" Hg :40C, and so on.  The problem is degree of impediment
>> >>> caused by the actual plastic.  To build off what Yuan-chia Joyce Koo
>> >>> has stated but with a different vector in mind, the plastic material
>> >>> of moisture bags for instance is highly resistant to diffusion.
>> >>> Different polymers will follow accordingly.
>> >>>
>> >>> For information, many plastics must be dried immediately prior to
>> >>> molding otherwise they suck up moisture like a sponge. Common
>> >>> hygroscopic polymers are Nylon, ABS (Acetyl Butyl Styrene), PC
>> >>> (Polycarbonate), and PMMA (Poly (methyl methacrylate)).  Nylon and
>> >>> PMMA are very common materials in component shells.  ABS and PC index*
>> >>> at temperatures not much higher than boiling water and are not
>> >>> typically used.  PP (Polypropylene) and PE
>> >>> (Polyethylene) are not so bad, hence their use in capacitors, but
>> >>> these index in the 200C range making them a bear for SMT placement.
>> >>> My general rule is the higher the MSL number, i.e., the more likely a
>> >>> part is to absorb moisture, the easier it is to dry.
>> >>>
>> >>> For normal bake (NO vacuum), here is the formula I derived several
>> >>> years
>> >>> ago:
>> >>> Thickness (mm) X Thickness (mm) (Divided by) Bake Temp Factor D125oC=
>> >>> 0.4427 // D90oC= 0.1270 // D40oC= 0.0131, Result is time in hours.
>> >>>
>> >>> I have never experimented with Vacuum Acceleration, but I will query
>> >>> the Penn State Plastics Engineering group with what we are trying to
>> >>> resolve and post those results to the J-STD-033 committee as well as
>> >>> here.
>> >>> * Index is the temperature at which a plastic flows well enough to be
>> >>> molded.  It is neither solid nor liquid, but soliquid.
>> >>>
>> >>> This all sounds like a job for Clumpy and Kloumpios when they are next
>> >>> available.
>> >>>
>> >>>
>>
>>
>> --
>> Steve Gregory
>> Kimco Design and Manufacturing
>> Process Engineer
>> (208) 322-0500 Ext. -3133
>>
>> --
>>
>>
>>
>> This email and any attachments are only
>> for use by the intended
>> recipient(s) and may contain legally privileged,
>>  confidential, proprietary
>> or otherwise private information. Any
>> unauthorized use, reproduction,
>> dissemination, distribution or other
>> disclosure of the contents of this
>> e-mail or its attachments is strictly
>>  prohibited. If you have received
>> this email in error, please notify the
>>  sender immediately and delete the
>> original.
>>
>
>


-- 
Steve Gregory
Kimco Design and Manufacturing
Process Engineer
(208) 322-0500 Ext. -3133

-- 



This email and any attachments are only 
for use by the intended 
recipient(s) and may contain legally privileged,
 confidential, proprietary 
or otherwise private information. Any 
unauthorized use, reproduction, 
dissemination, distribution or other 
disclosure of the contents of this 
e-mail or its attachments is strictly
 prohibited. If you have received 
this email in error, please notify the
 sender immediately and delete the 
original. 

ATOM RSS1 RSS2