I'm often asked by the production guys about risk of Au embrittlement, and
they show a board or a component which they suspect having too much of Gold.
The first test I use to practise takes 10 seconds to perform. I use a Faber
hard rubber pencil and give the board pads or the component terminal a few
hard strikes with the pencil. If the underlying nickel comes up immediately,
it's a good Au flash, and no risk of soldering. And most of the cases belong
to this group. I cannot recommend this 'method' to other than very
experienced ones.
(If I can go on striking the solder pad without seeing nickel, then I have
to do a more advanced examination of course.)
Inge
----- Original Message -----
From: "Gervascio, Thomas L" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, July 29, 2009 12:42 AM
Subject: Re: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT
> How could I get a copy of it? I thought EP&P was out of print..
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
> Sent: Tuesday, July 28, 2009 10:01 AM
> To: [log in to unmask]
> Subject: Re: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER
> JOINT
>
> Hi Jon - the folks from Lockheed published a very good article on the
> impact of gold on solder joints including the calculations/material
> parameters/graphs that would be useful to you. Pull a copy of this
> article: "Effects of Gold Diffusion on a Near Eutectic Solder Joint", S.
>
> Enwright, Electronic Packaging & Production, June 1998, pp 68-72. Good
> Luck.
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]
>
>
>
>
> "Roberts, Jon (SA-1)" <[log in to unmask]>
> Sent by: TechNet <[log in to unmask]>
> 07/28/2009 07:53 AM
> Please respond to
> TechNet E-Mail Forum <[log in to unmask]>; Please respond to
> "Roberts, Jon (SA-1)" <[log in to unmask]>
>
>
> To
> [log in to unmask]
> cc
>
> Subject
> [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT
>
>
>
>
>
>
> Does anyone have or know where to find the formula for determining the
> amount of percentage of gold in a SMT solder joint? Appreciate any
> help, Jon
>
>
> This communication is intended only for use by the addressee(s) named
> herein and may contain business confidential and/or legally privileged
> information. If you are not the intended recipient of this e-mail, you
> are
> hereby notified that any dissemination, distribution, disclosure or
> copying of this e-mail and its contents is strictly prohibited. If you
> have received this e-mail in error, kindly notify the sender by replying
>
> to this message. In addition, please permanently delete the message and
> any attachments without copying or disclosing the contents. Thank you
> for
> your cooperation.
> THIS DOCUMENT AND/OR SHIPMENT MAY CONTAIN COMMODITY ITEMS, SOFTWARE OR
> TECHNICAL DATA THAT IS CONTROLLED BY U.S. EXPORT LAW, AND MAY NOT BE
> EXPORTED OUTSIDE THE UNITED STATES OR TO NON U.S. PERSONS WITHOUT THE
> APPROPRIATE EXPORT LICENSE FROM EITHER THE U.S. DEPARTMENT OF STATE OR
> DEPARTMENT OF COMMERCE.
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text
> in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives
> Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask]
> or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text
> in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives
> Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
> ext.2815
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|