TECHNET Archives

October 2006

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Rich Wolbert <[log in to unmask]>
Date:
Wed, 18 Oct 2006 16:51:48 +0300
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Brian Ellis <[log in to unmask]>
Subject:
From:
Brian Ellis <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset=ISO-8859-1; format=flowed
MIME-Version:
1.0
Parts/Attachments:
text/plain (36 lines)
Use a water-soluble paste (with a good clean, of course).

Brian

Rich Wolbert wrote:
> OK, I know you guys are probably going to shake your head on this one, but
> I have to ask. We have a double sided fine pitch SMT assembly and we
> decided to go to white tin for the pad material. Here's where the problem
> comes in, we ran one side and when we started process the other side we
> found counterfeit chips. We stopped production for two weeks until the
> correct parts came in. When we tried to run the boards again, the PCB's
> oxidized so badly over the two weeks that we can not get the solder to
> wet. Any suggestions, other than scrapping the 170 assemblies at $600 a
> piece?
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2