TECHNET Archives

June 2002

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Paul Truit <[log in to unmask]>
Date:
Fri, 14 Jun 2002 15:56:20 -0400
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "Hogg, Blair K." <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
"Hogg, Blair K." <[log in to unmask]>
Parts/Attachments:
text/plain (79 lines)
Saw a similar problem with optocouplers a few years back (different
company). Turned out to be bad parts. Have you ruled this out, say by temp
cycling the component and testing after temp cycling? 

Blair Hogg
QA Manager 
GAI-Tronics

-----Original Message-----
From: Paul Truit [mailto:[log in to unmask]]
Sent: Friday, June 14, 2002 3:00 PM
To: [log in to unmask]
Subject: [TN] Optocoupler's


We are experiencing a problem related to an Optocoupler.  I wanted to
see if anyone had any ideas as to the whys.  The IC's have failed
intermittently in the field.

Specifics:
Mixed technology board.  The Opto in question is Through Hole.  It is
Hand inserted.  The board is processed using a VOC free OA flux that is
sprayed on with a spray fluxer. 2 bottom side convection pre-heaters
bring the board up to a 96°C (204°F) top side board temperature on a
conveyor that is set for 4'/min in a wave solder machine.  Wave solder
pot is at 260°C (500°F).  The maximum part lead temperature is
164°C(327°F) for 6 seconds. The board transitions into an aqueous
cleaner. The board has 6 feet to cool off before hitting the water.
This is 1.43 minutes. The water temp is set for 63°C(145°F). and the
belt speed is set for 4'/ min.  2 dryer sections dry the boards off.
Cooling of the part is a slope of -1.63°C/sec(-35°F/sec).

The optocoupler's pass a functional test.  They then fail intermittently
in the field.  Failure analysis of the IC has shown an inadequate die
bond between the Lead frame and the silicon die. 2 different date codes
have been found to have failed.

There has been a different EMS making a similar board using identical
part numbers that these boards have not failed.  What appears to be
different is we clean, they don't.  Any issues with aqueous cleaning and
Opto's? And this process causing the lead frame and die separation
issue?

--
Paul Truit, Mfg. Eng.
RBB Systems, Inc.
4265C E. Lincolnway
Wooster, OH  44691
Ph. (330) 567-2906 ext 514
Fax (330) 263-5324
Email: [log in to unmask]

----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2