Hi Dehoyos,
Most Kapton tapes have a silicone based adhesive. Silicon is a contaminant for AR and UR coatings and will not allow the coating to stick! We have different coating rooms for this purpose. One sprays AR and UR, while the other sprays only SR
Also we use a non silicone based adhesive for the masking we use with AR and UR
Amol Kane
M.S (Industrial Eng.)
Process Engineer
Harvard Custom Manufacturing, Inc.
941 Route 38 Owego, NY 13827
Phone: (607) 687-7669 x349
[log in to unmask]
www.harvardgrp.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dehoyos, Ramon
Sent: Thursday, June 22, 2006 11:47 AM
To: [log in to unmask]
Subject: Re: [TN] Conformal Coat Voids
You are having a case of dewetting. It happens with some kapton
dots. I have tried to cover them with UR coating and the coating pulls
away from the dot leaving the dot untouched no matter how many times I
brush the dots. There is also a ring around the dots where there is no
coating. It could be static build up or a chemical that rejects the
coating. Suggestion: after the board is totally cleaned, rinse it one
more time with DI. Submerge it in alcohol and brush the concerned areas.
Rinse it again with DI water, bake and then try to coat it. Second
suggestion: Place board in front of an Ion Generator for a few minutes.
Ramon
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bloomquist, Ken
Sent: Thursday, June 22, 2006 9:19 AM
To: [log in to unmask]
Subject: Re: [TN] Conformal Coat Voids
Hi Graham,
I have not noticed any dewetting anywhere else on these boards. There is
always a possibility that something could be coming out of the holes but
I'd think that it would get cooked away during wave solder or washed off
during cleaning.
Hi Amol,
We are doing some tests right now to see if there might be something in
the cleaning process. The flux is water soluble and the board gets run
through an inline washer two to three times during the process. The
board goes through one final saponified wash in a batch washer before
coating. We have not seen any residues on these solder joints after all
this cleaning.
What brought this to our attention was a test failure during a dust
test. It's a very difficult test with materials that are conductive.
We can apply a drop of water on the via's and create a failure of the
board so we know there's not much coating over the solder.
Is there any possibility that the really smooth slick domed surface is
allowing the coating to be pulled off of it?
Thanks,
KennyB
-----Original Message-----
From: Graham Naisbitt [mailto:[log in to unmask]]
Sent: Thursday, June 22, 2006 4:15 AM
To: [log in to unmask]
Subject: Re: [TN] Conformal Coat Voids
Hi Kenny
Clutching at straws here - any chance you have "drilling" residues
before the via is plated?
Can it be something from the via plating operation that has changed?
Have you noticed de-wetting anywhere other than the via's?
Regards
Graham Naisbitt
[log in to unmask]
Phone: +44 (0)12 5252 1500
Mobile: +44 (0) 79 6858 2121
______________________________________________________
Hi,
How are the boards cleaned before coating? For a test sample of boards,
take a Q-tip with a solvent like Xylene and manually scrub the problem
areas and then try the coating process. That way you can change the
cleaning procedure if necessary for those particular boards.
Amol Kane
M.S (Industrial Eng.)
Process Engineer
Harvard Custom Manufacturing
941 Route 38 Owego, NY 13827
Phone: (607) 687-7669 x349
[log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
CONFIDENTIALITY NOTICE:
This e-mail, and any attachments, is for the sole use of the intended
recipient(s) and may contain information that is confidential and
protected from disclosure under the law. Any unauthorized review, use,
disclosure, or distribution is prohibited. If you are not the intended
recipient, please contact the sender by reply e-mail, and delete/destroy
all copies of the original message and attachments.
Thank you.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|