The PCBs shops can inspect black pads using AOI (Orbotech, Camtec), what is
your tool?

Best  Regards

ROKAH Reuven




                      "Zweigart,
                      Siegmund"                  To:      [log in to unmask]
                      <SiegmundZweigart@         cc:
                      HG.SLR.COM>                Subject: [TN] Black Pad Detecting Machine
                      Sent by: TechNet
                      <[log in to unmask]
                      IPC.ORG>


                      19/08/2003 14:04
                      Please respond to
                      "TechNet E-Mail
                      Forum."; Please
                      respond to
                      "Zweigart,
                      Siegmund"





> Hi all,
>
> we are two students named Elisabeth Stumpf and Christian Wuerfel studying
> at Solectron Herrenberg in Germany.
> In the context of our studies we are currently working on a project to
> investigate the potential market for
> a machine which is designed by Solectron. This machine shall detect Black
> Pad infected PCBs before being assembled
> and without destruction of the PCB.
>
> The prototype is now under construction. Afterwards function tests will
be
> made, by which the operativeness of this machine
> is checked
>
> What is Black Pad?
>
> Black Pad is described as the corrosion of immersion gold-plated,
> elctroless nickel ( ENIG).
>
> Thereby interconnection failures occur after final assembly of the PCBs
> due to a poorly formed joint at the solder/nickel interface.
> When the suspect joint is stressed, the connection is easily broken,
> leaving an open cicuit.
> In other cases, the pads are dewetting during the soldering process.The
> dewetted pads are discolored black, which lead to the
> nomenclature BLack Pad.
>
> Investigations on Black Pad show that a corrosive interlayer between the
> gold and the nickel causes it. It is an insidious
> problem, since this interlayer is covered by gold and therefore, it has
> been not able until now to detect Black Pad by
> non-destructive methods. The symptoms of Black Pad only occcur after
> soldering which causes high costs since the PCB
> and the assembled componenets have to be scrapped.
>
>
> Elisabeth`s and my job is to decide if this machine can be successul.
> Therefore we need your support.
> If you are interested in our topic we would like to contact you
personally
> and ask you some questions.
> Of course we let you participate in our results.
>
> We would be very grateful for your answers!
> Thanks a lot in advance.
>
> Elisabeth and Christian
>
>

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2