TECHNET Archives

September 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
"Dehoyos, Ramon" <[log in to unmask]>
Date:
Thu, 16 Sep 2004 05:54:28 -0700
MIME-Version:
1.0
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Dehoyos, Ramon" <[log in to unmask]>
Parts/Attachments:
text/plain (257 lines)
        Hi Bryan:
         Are you using low flux solder? Are the terminal old and have lots of oxide? When you replated the terminals, did you get rid of the problem? Have you tried to solder this terminals on other type of boards?
        Regards,
        Ramon

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of David D. Hillman
Sent: Wednesday, September 15, 2004 6:50 PM
To: [log in to unmask]
Subject: Re: [TN] HMP Solder Joint Cracking


Hi Bryan! One possible root cause to explore is that the "cracks" you have
observed are actually shrinkage voids/cavities that intercept the solder
joint surface. There have been several studies (NIST, NCMS) that have show
that the high tin content solder alloys can form small shrinkage cavities
that terminate at the solder joint surface. These shrinkage cavities could
easily be mistaken for cracks. I recommend you microsection one of the
suspect solder joints to see if you have a crack or a shrinkage cavity.
Good Luck.

Dave Hillman
Rockwell Collins
[log in to unmask]




                      "Kerr, Bryan"
                      <bryan.kerr@AMSJV        To:       [log in to unmask]
                      .COM>                    cc:
                      Sent by: TechNet         Subject:  Re: [TN] HMP Solder Joint Cracking
                      <[log in to unmask]>


                      09/15/2004 10:27
                      AM
                      Please respond to
                      TechNet E-Mail
                      Forum; Please
                      respond to "Kerr,
                      Bryan"






The cracks occur immediately on alloy solidification - I've watched it
happen under a scope. Can't be sure that some don't occur later but that is
a worrying thought which could affect reliability.

Cheers

Bryan

-----Original Message-----
From: Marsico, James [mailto:[log in to unmask]]
Sent: 15 September 2004 16:21
To: 'Kerr, Bryan'
Subject: RE: [TN] HMP Solder Joint Cracking


When are the cracks occurring?  Ate the assemblies thermally stressed after
the terminals are soldered?  Do the cracks occur after a wire is soldered
to
the turrets?

Jim Marsico
Senior Engineer
Production Engineering
EDO Electronics Systems Group
[log in to unmask] <mailto:[log in to unmask]>
631-595-5879



        -----Original Message-----
        From:   Kerr, Bryan [SMTP:[log in to unmask]]
        Sent:   Wednesday, September 15, 2004 11:07 AM
        To:     'Marsico, James'; IPC Mailing List (E-mail)
        Subject:        RE: [TN] HMP Solder Joint Cracking


        Thanks Jim

        We are seeing some of the edge solderability issues that you
mention
however
        there is definite cracking as shown in microsections done by
ourselves.
        Another batch of pins has better solderability at the edge however
we still
        get cracks occurring.

        Cheers

        Bryan

        -----Original Message-----
        From: Marsico, James [mailto:[log in to unmask]]
        Sent: 15 September 2004 16:04
        To: 'TechNet E-Mail Forum'; 'Kerr, Bryan'
        Subject: RE: [TN] HMP Solder Joint Cracking


                       *** WARNING ***

        This mail has originated outside your organization,
        either from an external partner or the Global Internet.
             Keep this in mind if you answer this message.

        We've seen this problem in the past.  The main culprit, in our
case,
was the
        solderability of the terminal on the corner of the swaged area.
What looks
        like a crack may be an unsolderable line around the periphery of
the
swaged
        area.  Try dipping the swaged end of a terminal into a solder pot
and see if
        the corner edge wets.

        Jim Marsico
        Senior Engineer
        Production Engineering
        EDO Electronics Systems Group
        [log in to unmask] <mailto:[log in to unmask]>
        631-595-5879



                -----Original Message-----
                From:   Kerr, Bryan [SMTP:[log in to unmask]]
                Sent:   Wednesday, September 15, 2004 10:35 AM
                To:     [log in to unmask]
                Subject:        [TN] HMP Solder Joint Cracking

                Hi

                We are fitting a swaged turret terminal and soldering using
96% Tin
        4%
                Silver alloy and have experienced cracks running around the
edge of
        the
                swage solder joint - between the pin and the solder.
Re-soldering
        gets rid
                of it in most but not all cases. I have thought that
perhaps
some
        stress
                relaxation is occurring in the swage area (brass base
material)
        during
                soldering resulting in these cracks.
                Can anyone shed any light on this problem ?

                Cheers

                Bryan Kerr
                Principal Quality Engineer
                Process and Materials Laboratory
                AMS Hillend



********************************************************************
                This email and any attachments are confidential to the
intended
                recipient and may also be privileged. If you are not the
intended
                recipient please delete it from your system and notify the
sender.
                You should not copy it or use it for any purpose nor
disclose or
                distribute its contents to any other person.

********************************************************************

                ---------------------------------------------------
                Technet Mail List provided as a service by IPC using
LISTSERV 1.8e
                To unsubscribe, send a message to [log in to unmask] with
following
        text in
                the BODY (NOT the subject field): SIGNOFF Technet
                To temporarily halt or (re-start) delivery of Technet send
e-mail to
        [log in to unmask]: SET Technet NOMAIL or (MAIL)
                To receive ONE mailing per day of all the posts: send
e-mail
to
        [log in to unmask]: SET Technet Digest
                Search the archives of previous posts at:
        http://listserv.ipc.org/archives
                Please visit IPC web site
        http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information,
        or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
                -----------------------------------------------------


********************************************************************
        This email and any attachments are confidential to the intended
        recipient and may also be privileged. If you are not the intended
        recipient please delete it from your system and notify the sender.
        You should not copy it or use it for any purpose nor disclose or
        distribute its contents to any other person.

********************************************************************

********************************************************************
This email and any attachments are confidential to the intended
recipient and may also be privileged. If you are not the intended
recipient please delete it from your system and notify the sender.
You should not copy it or use it for any purpose nor disclose or
distribute its contents to any other person.
********************************************************************

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2