Yup! CR = Convection Reflow Soldering. Darn! I'm developing the local habit
of using acronyms without explaning them!
I can give you some chapter and verse on hole diameters and aspect ratios
that are successful or not, if you want. I've had 24 mil diameter holes
filled that are only 7 mils deep, and as small as 18 mils with a 4:1 aspect
ratio. I think about 12 mils at this ratio is the lower limit (certainly
with my fab shops), and 25 mils is about the upper limit if you want to
maintain a reasonably flat finish. with larger diameters, the material
tends to sag and you get dips on one side and bumps on the other. We had to
experiment a bit with hole sizes outside of this range to see what was
possible and what was not.
Depending on the application, though, I have come to realise that the
process is more trouble than it's worth most of the time.
Peter
Steve Gregory <[log in to unmask]> 15/11/2002 08:59 AM
Sent by: TechNet <[log in to unmask]>
Please respond to "TechNet E-Mail Forum."; Please respond to SteveZeva
To: [log in to unmask]
cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST Aero/ST Group)
Subject: Re: [TN] Conductive epoxy via filling...
Hi Peter!
I just want to ask a question about your statement below:
It was also a compromise solution to filling all the holes with solder,
which
may have fallen out again during CR,
What is CR? Convection reflow?
-Steve-
--------------------------------------------------- Technet Mail List
provided as a free service by IPC using LISTSERV 1.8e To unsubscribe, send
a message to [log in to unmask] with following text in the BODY (NOT the
subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery
of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To
receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest Search the archives of previous posts
at: http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/html/forum.htm for additional information, or contact
Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|