Phil: Plating on aluminum is not an easy task. The typical process is:
1. Alkaline clean
2. Acid desmut
3. Zincate 1
4. Nitric acid dip
5. Zincate 2
Then overplate with a copper strike electroplate or electroless nickel.
Since the die is "singulated" I don't think you can go the copper electroplate
route, which leaves the electroless nickel(not the easiest process to control).
The solder coating would follow. I believe there is no way you can solder dip
directly to the zincate and assure a good bond.
This application requires a lot of chemistry and control. I would not recommend
it unless you have a good background in plating and process control. Good Luck!
regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett Wa.
425-356-6076
On Mon, 29 Mar 1999 08:33:44 -0800 Phil Hersey wrote:
> From: Phil Hersey <[log in to unmask]>
> Date: Mon, 29 Mar 1999 08:33:44 -0800
> Subject: [TN] zincate dip for solder bumping?
> To: [log in to unmask]
>
> Does anyone know anything about "zincate" dip for sensitizing aluminum for
> electroplating? Atotech has such a bath and evidently it makes aluminum
> plateable. If so, I can envision a process to solder bump even already
> singulated die by zincating the bond pads and then solder dipping.
>
> Resp.
> Phil Hersey, Carson City Nevada USA
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
> ################################################################
>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|