TECHNET Archives

June 2007

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Mime-Version:
1.0
Sender:
X-To:
Date:
Tue, 5 Jun 2007 09:10:26 -0700
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Dwight Mattix <[log in to unmask]>
Subject:
From:
Dwight Mattix <[log in to unmask]>
In-Reply-To:
<OFB33524A6.5E217A9C-ON852572F1.0055AB84-852572F1.0055E5BA@ ltx.com>
Content-Type:
text/plain; charset="us-ascii"; format=flowed
Parts/Attachments:
text/plain (109 lines)
At 08:38 AM 6/5/2007, Kerry McMullen wrote:
>Hi Tom,
>Check the plating spec on the fab.   The plating thickness in the via's
>should be specified at 0.001" absolute minimum if you are going with LF
>processes, regardless of the board material.
>  (That is what I am told).

Class 2, 0.0008" minimum on PTH has been fine in our IST Pb-free qual 
work.  Quality of drill/roughness, hole prep, electroless Cu 
grain/porosity, and electrolytic Cu ductility is much more important.

>  I
>have made this change on my large 18+ layer boards, and my quality/yields
>have increased, and my opens have practically diappeared.
>
>Kerry McMullen
>Principal New Product Mfg. Engineer
>LTX Corporation
>825 University Avenue
>Norwood, MA 02062-2643
>(T) 781-467-5468
>(C) 508-631-1832
>(F) 781-461-0993
>
>
>
>Tom Parkinson <[log in to unmask]>
>Sent by: TechNet <[log in to unmask]>
>06/05/2007 10:13 AM
>Please respond to
>TechNet E-Mail Forum <[log in to unmask]>; Please respond to
>Tom Parkinson <[log in to unmask]>
>
>
>To
>[log in to unmask]
>cc
>
>Subject
>[TN] Via Open
>
>
>
>
>
>
>Tech Net & Designer Net
>
>Greetings. We are running into a situation on Lead Free processed PCBs.
>Failure mode is finding open vias during unit testing (fully populated).
>
>Boards are Tg170, Material type EM320, 0.063" thick boards.
>6 layers of 1 oz copper. ENIG 3~5u"
>
>Suspect vias go from top layer to bottom layer only.
>
>After running through reflow, we have found vias open. No visual signs of
>delamination, however when ohming out the via, if we press on the via we
>get
>continuity - thus we suspect the vias are opening during the process.
>
>Anyone out there having these problems, or information concerning this
>failure mode?  Z-expansion failure?
>
>
>Tom Parkinson
>Quality System Manager - CIT
>WinTronics, Inc.
>Phone: 724-981-5770 - extension 235
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
>
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to 
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to 
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
>for additional information, or contact Keach Sasamori at [log in to unmask] or 
>847-615-7100 ext.2815
>-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2