Ted,
Our company has done a little compatibility testing between previously
approved fluxes and never found a failure. Note, I mentioned that the
fluxes were previously approved. By this I mean that they have passed the
chloride ion, copper mirror, SIR and electromigration requirements of
Bellcore GR-78-CORE. In addition the latter was done with stripes of
various solder masks across the coupons as we have found some mask/flux
incompatibilities. This flux/mask testing we do for all chemicals that are
going to come in contact with the bare PCB or the completed PCBA. However,
as far as doing a complete matrix of all fluxes with every board vendor
source of a particular mask or a matrix of all flux combinations, we
wouldn't even try that nightmare - too many combinations.
For SIR the Bellcore test is 96 hours and I think the IPC test is 7 days and
the Bellcore electromigration test is 500 hours (~4 weeks). An 8 week SIR
test? I am not familiar with this one. My store of Circuit Assembly mags
does not stretch back to 1992.
regards,
Bev Christian
Materials Engineering Lab
Carrier Solutions
Nortel Networks
613-967-5407
> -----Original Message-----
> From: Ted Labowski [SMTP:[log in to unmask]]
> Sent: Tuesday, March 02, 1999 9:45 AM
> To: [log in to unmask]
> Subject: [TN] No Clean Flux Compatability
>
> My company is making a slow transition to No Clean chemistry in our SMT,
> Wave, and Post Wave operations.
>
> We are taking a systematic approach and thought we were on a smooth
> path until I ran across a June 1992 article published in Circuit
> Assembly and authored by several Engineers at the Foxboro Company
> (Foxboro, MA).
>
> The article was written specifically about No Clean materials and it
> warns about "incompatibilities between similar solder flux products
> supplied by different vendors." The conclusion is rather frightening
> "The potential for intermittent and ultimately catastrophic failure of a
> circuit over time due to flux incompatibility is cause for serious
> concern."
>
> I have contacted several industry experts and all downplay the
> significance of compatibility issues, although none have performed
> independent testing to qualify their "opinions".
>
> Does anyone have any first hand experience with No Clean flux
> incompatibilities? Additionally, is there any material published on
> this subject other than the one I ran across?
>
> Barring any new information, I am prepared to undertake a regimen of
> testing which will verify the compatibility of the No Clean materials
> which are currently approved by MPI. The testing will be similar to
> that performed in the Foxboro article ( SIR using IPC-B-25 coupons, 40
> degrees C/95% RH, 30 V bias, measured incrementally during the 8 week
> cycle).
>
>
> Ted Labowski
> Vice President - Quality
> Microboard Processing, Inc.
>
> Email : [log in to unmask]
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
> section for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or
> 847-509-9700 ext.312
> ################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|