In general, the 7628 prepreg comes in either a low, standard or high resin
content. This same resin content variation can also be applied to other
glass styles, such as 2116, 1080 etc. It is very much dependant on what
volumes are required by the fabricator, which would justify the production
run by the laminator.
"B" stage is simply the resin state, which in prepreg format is the tack
dried resin system, capable of going through a rheology curve in the press,
which then melts, encapsulates and sets to a solid "C" stage irreversible
cured state.
Polyclad are one such supplier, who can offer 7628 with a 43% rc standard
and 48% high rc. I have found that it is usually the fabricator who
specifies a higher rc, when he has free reign on the build of the panel, and
this is normally for cost, where one ply of high rc 7628 replaces 2 plies of
2116 etc.
Only concern is where the fabricators have a fair amount of encapsulation to
achieve, either by via hole filling or high copper weights. When using high
rc products, it is also best to use vacuum lamination where possible.
Regards,
Colin McVean
Circuit Manufacture Ltd
Unit 9-12
Rowleys Green Lane
Longford
Coventry
CV6 6AG
Tel: 02476 666168
Fax: 02476 637089
________________________________________________
This email is confidential and intended solely for the use
of the individual to whom it is addressed. Any views or
opinions presented are solely those of the author and do
not necessarily represent those of the Company.
If you are not the intended recipient, be advised that you
have received this email in error and that any use,
dissemination, forwarding, printing, or copying of this
email is strictly prohibited.
If you have received this email in error please notify the
Company by telephone on +44 (0)24 7666 6168 or reply
by email to the sender and delete the email.
________________________________________________
Whilst every effort has been made to ensure that there are
no viruses embedded in this email, we highly recommend
that you virus scan any attached files using your own anti-
virus software.
-----Original Message-----
From: Tom Bresnan [mailto:[log in to unmask]]
Sent: Wednesday, May 19, 2004 5:16 AM
To: [log in to unmask]
Subject: Re: [TN] FW: [DC] Core Constructions
Let me also add that lead-time may increase as well as cost. Be sure you
absolutely 'need' the material. Most fab houses won't have it on the shelf
(can't anticipate every customer's needs) and there may be minimum run costs
incurred as well. Work with your board vendor(s) to come up with a standard
material stackup to lessen the impacts.
-----Original Message-----
From: Jeffrey Bush [mailto:[log in to unmask]]
Sent: Tuesday, May 18, 2004 4:17 PM
To: [log in to unmask]
Subject: Re: [TN] FW: [DC] Core Constructions
You are able to get higher resin contents from most laminate suppliers.
They will have a part listing of standard glass styles with varying
resin contents. Increasing the resin content in usually done to solve
an issue like poor wet-out of the glass, or voiding due to thicker
copper. Generally thickness yield per ply will increase with the RC, as
will the cost.
Jeffrey Bush
Director, Quality Assurance and Technical Support
76 Technology Drive - POB 1890
Brattleboro, Vermont 05302-1890
Tel. 802.257.4571.21 Fax. 802.257.0011
[log in to unmask]
http://www.vtcircuits.com
-----Original Message-----
From: Brooks,Bill [mailto:[log in to unmask]]
Sent: Tuesday, May 18, 2004 3:50 PM
To: [log in to unmask]
Subject: [TN] FW: [DC] Core Constructions
Is there a materials expert out there that can answer Mike's question
below?
B-stage epoxy resin is somewhat of a mystery to many designers. Perhaps
someone can clarify the reference to "High Resin Content" as apposed to
? what other options are available and how they affect the construction
of the FR4 board. Please copy to the group too so we can all learn from
this.
Bill Brooks
PCB Design Engineer , C.I.D., C.I.I.
Tel: (760)597-1500 Ext 3772 Fax: (760)597-1510 http://pcbwizards.com
-----Original Message-----
From: Mike Valle [mailto:[log in to unmask]]
Sent: Tuesday, May 18, 2004 12:24 PM
To: [log in to unmask]
Subject: [DC] Core Constructions
Hi, I need some help trying to find some information on FR-4
construction and thickness. I've come across a 4-layer stackup on a
cross-section detail on one of our drawings and I can't seem to find it
in IPC-4121. Our b-stage construction calls out for 1 ply of b-stage HRC
(high resin content) 7628 .0068. Another detail on another drawing calls
out for 1 ply of b-stage HRC (high resin content) 7628 .008. What I've
been finding in IPC-4121 is that there is a FR-4 11 (7.087) 7628 40% RC
and a HFR-4 11 (7.087) 40% RC, which is a high tg. So, my question is -
is there such a thing as HRC - high resin content with varying
thicknesses?
Thanks,
Mike Valle
Project Engineer, PCB Design
Shure Inc.
(847)424-4616
[log in to unmask]
------------------------------------------------------------------------
----
-----
DesignerCouncil Mail List provided as a free service by IPC using
LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with
following text in the BODY (NOT the subject field): SIGNOFF
DesignerCouncil. To set a vacation stop for delivery of DesignerCouncil
send: SET DesignerCouncil NOMAIL Search previous postings at:
www.ipc.org > On-Line Resources & Databases > E-mail Archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-509-9700 ext.5315
------------------------------------------------------------------------
----
-----
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|