TECHNET Archives

October 2000

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Mime-Version:
1.0
Sender:
Subject:
From:
Guenter Grossmann <[log in to unmask]>
Date:
Mon, 30 Oct 2000 16:32:42 +0100
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset=ISO-8859-1
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Guenter Grossmann <[log in to unmask]>
Parts/Attachments:
text/plain (43 lines)
The time necessary for the relaxation of elastically stored deformation depends on the temperature as well as on the temperature gradient. Since the creep rate depends on temperature and stress the relaxation is a asymptotic process that leaves always a remaining amount of strain to be induced into the solder joint after a certain dwell time. However this remaining strain becomes negligible if the dwell time is sufficiently small. We did some calculations for ceramic chip capacitors 2220 on 1.6mm FR4 with a plastically deformed layer of 30um based on our deformation model for Sn62Pb36Ag2. I have the feeling that these calculations are quite a good guideline to estimate the dwell times necessary to leave a certain remaining strain to total relaxation in various applications.

In the case of 125°C I am sure that a dwell time of 5 Minutes after the specimen has reached the 125°C is sufficient to have less than 0.04 % remaining strain.
At -55°C The creep behaviour of Sn62Pb36Ag2 is quite slow. In my opinion the following dwell times are necessary:

Remaining strain    Temperature gradient     Dwell time 

0.1%                             2°C/min.                         5min
0.06%                           2°C/min                        50min
0.04%                           2°C/min                      170min

0.1%                             10°C/min                      15 min
0.06%                           10°C/min                     150min
0.04%                           10°C/min                   >500min

0.1%                             40°C/min                     350min

I didn't calculate any further  since the dwell times for small amounts of remaining strain at 40°C/min and faster become very long. You can find these data as a graph for 2, 10, 40 and 80°C/min in the  proceedings of the 1997  IEMT symposium in Austin TX.


Have a great day

Guenter

Guenter Grossmann
Swiss Federal Institute for Materials Testing and Research EMPA
Centre for Reliability
8600 Duebendorf
Switzerland

Phone: xx41 1 823 4279
Fax :      xx41 1823 4054
mail:     [log in to unmask]

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2