If x-ray is not an option, you need to set up a soldering process that would not require inspection. On a thermally relieved pad that does not get sufficient fill, you need to preheat the pad area prior to hand soldering to compensate for the heat sinking. If you can get a dummy populated board, preheat it to a known reference level, and then remove the connector body to examine the % fill. Find the minimum reference preheat that will obtain your desired % fill. If you can't get a dummy populated board, you can use a few production boards to find the reference preheat by utilizing an ouitside x-ray service to determine the % fill.
>>> [log in to unmask] 2/28/2006 7:55 AM >>>
We are having a heck of a time inspecting some solder joints and could
use your help.
Per Class 3 a solder joint is supposed to have at least a 75% fill. We
have a circuit board that has large ground planes and hand soldered
connectors that are impossible to inspect for top side solder.
We do not have access to an x-ray and are wondering if there are any
clever ways to inspect these solder joints.
Thanks,
KennyB
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|